MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECANAT® GF20 natural PC, 20% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, 20% Glass Filled

Material Notes:
  • high toughness
  • good thermal stability
  • very high stiffness
  • good tensile strength
Target Industries:
  • aircraft and aerospace technology
  • automotive industry
  • fixture construction
  • electrical engineering
  • mechanical engineering

Information provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.33 g/cc0.0480 lb/in³
Moisture Absorption 0.290 %0.290 %saturation; ASTM D570
 0.0700 %
@Time 86400 sec
0.0700 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8787ASTM D 785
Tensile Strength, Yield 75.8 MPa11000 psiASTM D 638
Elongation at Break 3.0 %3.0 %ASTM D 638
Modulus of Elasticity 4.83 GPa700 ksiASTM D 638
Flexural Strength 115 MPa16700 psiASTM D 790
Flexural Modulus 4.14 GPa600 ksiASTM D 790
Compressive Yield Strength 103 MPa
@Strain 10 %
15000 psi
@Strain 10 %
ASTM D 695
Compressive Strength 13.8 MPa
@Strain 1 %
2000 psi
@Strain 1 %
ASTM D 695
Compressive Modulus 2.20 GPa319 ksiASTM D 695
Izod Impact, Unnotched 1.10 J/cm2.06 ft-lb/in
Coefficient of Friction, Dynamic 0.22
@Pressure 0.276 MPa
0.22
@Pressure 40.0 psi
50 fpm; ASTM D 3702
K (wear) Factor 242 x 10-8 mm³/N-M120 x 10-10 in³-min/ft-lb-hrAgainst Steel, 40 psi, 50 fpm; ASTM D 3702
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+17 ohm-cm1.00e+17 ohm-cmASTM D 257
Dielectric Constant  3.13
@Frequency 1e+6 Hz
3.13
@Frequency 1e+6 Hz
ASTM D 150
 3.17
@Frequency 60 Hz
3.17
@Frequency 60 Hz
50% RH; ASTM D 150
Dielectric Strength 19.3 kV/mm490 kV/inASTM D 149
Dissipation Factor 0.00090
@Frequency 60 Hz
0.00090
@Frequency 60 Hz
ASTM D 150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 27.0 µm/m-°C
@Temperature -40.0 - 95.0 °C
15.0 µin/in-°F
@Temperature -40.0 - 203 °F
ASTM E 831
Maximum Service Temperature, Air 130 °C266 °FLong Term
 135 °C275 °FIntermittent
Deflection Temperature at 0.46 MPa (66 psi) 148 °C298 °FASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 146 °C295 °FASTM D 648
Vicat Softening Point 165 °C329 °FASTM D1525
Flammability, UL94 V-0V-0
 
Descriptive Properties
Colorblue grey opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENSIN8173 / 319101

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.