MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Gougeon Brothers PRO-SET® HTP 182/HTP 286 High-Temp Laminating Epoxy
Categories: Polymer; Thermoset; Epoxy

Material Notes: High-temperature, high-performance epoxy formulation for synthetic composite part and tooling manufacture.
Tg as high as 300°F (149°C) with proper post cure. Provides excellent temperature stability and great part cosmetics.
Slow cure speed hardener provides 4 to 5 hours working time at 72°F (22°C). A typical laminate will gel in 8 to 10 hours at room temperature.
Medium viscosity for wet out of synthetic composite fabrics.
Elevated temperature cure is required. Parts can be pulled after 24-48 hours at room temperature or sooner after a mild initial cure of 90-110°F (32-43°C). See chart for post cure information.
Quality-control tinting is available at no extra charge; simply add "QC" after the product code on your order.

Information provided by Gougeon Brothers, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.980 g/cc0.0354 lb/in³Hardener
 1.16 g/cc0.0419 lb/in³Cured
 1.17 g/cc0.0423 lb/in³Resin
Viscosity  180 cP
@Temperature 22.0 °C
180 cP
@Temperature 71.6 °F
hardener; ASTM D2196
 250 cP
@Temperature 48.9 °C
250 cP
@Temperature 120 °F
Mixed
 1500 cP
@Temperature 29.4 °C
1500 cP
@Temperature 84.9 °F
Mixed
 3000 cP
@Temperature 29.0 °C
3000 cP
@Temperature 84.2 °F
Mixed; ASTM D2196
 6600 cP
@Temperature 15.6 °C
6600 cP
@Temperature 60.1 °F
Mixed
 8200 cP
@Temperature 22.0 °C
8200 cP
@Temperature 71.6 °F
resin; ASTM D2196
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 9494RT + 60°C x 2hr + 135°C x 12hr; ASTM D2240
Tensile Strength 62.1 MPa9000 psiRT + 60°C x 2hr + 135°C x 12hr; ASTM D638
Elongation at Break 3.8 %3.8 %RT + 60°C x 2hr + 135°C x 12hr; ASTM D638
Tensile Modulus 2.82 GPa409 ksiRT + 60°C x 2hr + 135°C x 12hr; ASTM D638
Flexural Strength 111 MPa16100 psiRT + 60°C x 2hr + 135°C x 12hr; ASTM D790
Flexural Modulus 2.76 GPa400 ksiRT + 60°C x 2hr + 135°C x 12hr; ASTM D790
Compressive Yield Strength 103.9 MPa15070 psiRT + 60°C x 2hr + 135°C x 12hr; ASTM D695
 
Thermal PropertiesMetricEnglishComments
CTE, linear  53.68 µm/m-°C
@Temperature -30.0 - 30.0 °C
29.82 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM E831
 81.0 µm/m-°C
@Temperature 30.0 - 120 °C
45.0 µin/in-°F
@Temperature 86.0 - 248 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 143 °C289 °FRT + 60°C x 2hr + 135°C x 12hr; ASTM D648
Glass Transition Temp, Tg 152 °C306 °FRT + 60°C x 2hr + 135°C x 12hr, DMA Onset Storage Modulus, 1 Hz, 3°C per minute; ASTM E1640
 153 °C307 °FRT + 60°C x 2hr + 135°C x 12hr, DSC Onset– 1st Heat; ASTM E1356
 165 °C329 °FRT + 60°C x 2hr + 135°C x 12hr, DMA Peak Tan Delta, 1 Hz, 3°C per minute; ASTM E1640
 
Processing PropertiesMetricEnglishComments
Cure Time 480 - 600 min8.00 - 10.0 hourtypical laminate will be gelled
Pot Life  75.0 min
@Load 0.500 kg
75.0 min
@Load 1.10 lb
ASTM D2471
 100 min
@Load 0.150 kg
100 min
@Load 0.331 lb
ASTM D2471
Working Life 240 - 300 min240 - 300 min
Shelf Life 18.0 Month18.0 Monthhardener
 36.0 Month36.0 Monthresin
 
Descriptive Properties
Mix ratio100:18.1 - 100:23.9Weight Range, Resin: Hardener
 100:20.9Weight, Resin: Hardener
 100:21.6 - 100:28.5Volume Range, Resin: Hardener
 100:25.0Volume, Resin: Hardener
 4.00:1Volume, Resin: Hardener
 4.64:1 - 3.51:1Volume Range, Resin: Hardener
 4.70:1Weight, Resin: Hardener
 5.54:1 - 4.19:1Weight Range, Resin: Hardener

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PGOUGP946 / 290789

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.