MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Overview of materials for Polyamide-Imide, Molded
Categories: Polymer; Thermoplastic; Polyamide-imide (PAI); Polyamide-Imide, Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyamide-Imide, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.40 - 1.58 g/cc0.0506 - 0.0571 lb/in³Average value: 1.47 g/cc Grade Count:7
Water Absorption 0.200 - 0.600 %0.200 - 0.600 %Average value: 0.332 % Grade Count:6
Water Absorption at Saturation 1.50 - 4.60 %1.50 - 4.60 %Average value: 2.20 % Grade Count:5
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 70.0 - 80.070.0 - 80.0Average value: 75.3 Grade Count:3
Hardness, Rockwell M 106 - 119106 - 119Average value: 113 Grade Count:5
Hardness, Shore D 90.090.0Average value: 90.0 Grade Count:4
Tensile Strength, Ultimate 62.1 - 122 MPa9000 - 17700 psiAverage value: 94.8 MPa Grade Count:7
 53.0 - 53.0 MPa
@Temperature 235 - 235 °C
7690 - 7690 psi
@Temperature 455 - 455 °F
Average value: 53.0 MPa Grade Count:1
Elongation at Break 2.00 - 6.40 %2.00 - 6.40 %Average value: 3.39 % Grade Count:7
Modulus of Elasticity 3.03 - 5.52 GPa440 - 800 ksiAverage value: 3.94 GPa Grade Count:6
Flexural Yield Strength 89.6 - 165 MPa13000 - 24000 psiAverage value: 135 MPa Grade Count:7
 71.0 - 71.0 MPa
@Temperature 235 - 235 °C
10300 - 10300 psi
@Temperature 455 - 455 °F
Average value: 71.0 MPa Grade Count:1
Flexural Modulus 3.79 - 5.66 GPa550 - 821 ksiAverage value: 4.53 GPa Grade Count:7
Compressive Yield Strength 31.0 - 200 MPa4500 - 29000 psiAverage value: 132 MPa Grade Count:6
 64.0 - 64.0 MPa
@Temperature 235 - 235 °C
9280 - 9280 psi
@Temperature 455 - 455 °F
Average value: 64.0 MPa Grade Count:1
Compressive Modulus 2.41 - 3.50 GPa350 - 508 ksiAverage value: 2.80 GPa Grade Count:6
Izod Impact, Notched 0.267 - 0.801 J/cm0.500 - 1.50 ft-lb/inAverage value: 0.521 J/cm Grade Count:6
Coefficient of Friction 0.200 - 0.3000.200 - 0.300Average value: 0.235 Grade Count:4
K (wear) Factor 302 - 1010 x 10-8 mm³/N-M150 - 500 x 10-10 in³-min/ft-lb-hrAverage value: 637 x 10-8 mm³/N-M Grade Count:4
Limiting Pressure Velocity 0.140 - 0.946 MPa-m/sec4000 - 27000 psi-ft/minAverage value: 0.497 MPa-m/sec Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1.00e+10 - 1.00e+13 ohm1.00e+10 - 1.00e+13 ohmAverage value: 8.10e+12 ohm Grade Count:5
Dielectric Constant 3.34 - 6.003.34 - 6.00Average value: 4.54 Grade Count:5
Dielectric Strength 13.7 - 23.6 kV/mm348 - 600 kV/inAverage value: 18.4 kV/mm Grade Count:4
Dissipation Factor 0.00500 - 0.1820.00500 - 0.182Average value: 0.0411 Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 27.0 - 50.4 µm/m-°C15.0 - 28.0 µin/in-°FAverage value: 37.7 µm/m-°C Grade Count:6
Thermal Conductivity 0.259 - 0.533 W/m-K1.80 - 3.70 BTU-in/hr-ft²-°FAverage value: 0.389 W/m-K Grade Count:4
Maximum Service Temperature, Air 260 °C500 °FAverage value: 260 °C Grade Count:5
Deflection Temperature at 1.8 MPa (264 psi) 257 - 279 °C494 - 534 °FAverage value: 273 °C Grade Count:5
Glass Transition Temp, Tg 275 - 280 °C527 - 536 °FAverage value: 276 °C Grade Count:6
Flammability, UL94 V-0V-0Grade Count:6

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyetheretherketone, PEEK, Aramid Fiber Filled
Overview of materials for Polyamide-Imide, Glass Filled
Bamberger Polymers Bapolene® EVA-1120 Ethylene Vinyl Acetate (EVA)
Overview of materials for Polyimide
Overview of materials for Polycarbonate/ABS Alloy, Glass Fiber Filled

O2800 / 78112

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.