E-Glass Fiber, Generic
Categories: Ceramic; Glass; Glass Fiber; Oxide; Silicon Oxide; Other Engineering Material; Composite Fibers

Material Notes: Used as a reinforcing agent in fiber glass composites, including biomedical/surgical applications.

Information provide by Owens Corning and the reference(s).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.54 - 2.60 g/cc0.0918 - 0.0939 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  521 MPa
@Temperature -190 °C
75500 psi
@Temperature -310 °F
 1725 MPa
@Temperature 540 °C
250200 psi
@Temperature 1000 °F
 2620 MPa
@Temperature 370 °C
380000 psi
@Temperature 698 °F
 3450 - 3790 MPa
@Temperature 22.0 °C
500000 - 550000 psi
@Temperature 71.6 °F
Virgin strength
Elongation at Break 4.8 %4.8 %
Modulus of Elasticity 72.4 GPa10500 ksi
 72.3 GPa
@Temperature 540 °C
10500 ksi
@Temperature 1000 °F
Poissons Ratio 0.200.20
Shear Modulus 30.0 GPa4350 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 4.02e+12 ohm-cm4.02e+12 ohm-cm
Dielectric Constant  5.9 - 6.4
@Frequency 60 Hz
5.9 - 6.4
@Frequency 60 Hz
 6.3 - 6.6
@Frequency 1e+6 Hz
6.3 - 6.6
@Frequency 1e+6 Hz
Dielectric Strength 10.3 kV/mm262 kV/in
Dissipation Factor  0.0025
@Frequency 1e+6 Hz
0.0025
@Frequency 1e+6 Hz
 0.0034
@Frequency 60 Hz
0.0034
@Frequency 60 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear  5.00 µm/m-°C
@Temperature 20.0 °C
2.78 µin/in-°F
@Temperature 68.0 °F
 5.40 µm/m-°C
@Temperature -30.0 - 250 °C
3.00 µin/in-°F
@Temperature -22.0 - 482 °F
Specific Heat Capacity  0.810 J/g-°C
@Temperature 23.0 °C
0.194 BTU/lb-°F
@Temperature 73.4 °F
 1.03 J/g-°C
@Temperature 200 °C
0.246 BTU/lb-°F
@Temperature 392 °F
Thermal Conductivity 1.30 W/m-K9.02 BTU-in/hr-ft²-°F
Melting Point <= 1725 °C<= 3137 °F
Softening Point 840.6 °C1545 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5581.558
 1.5621.562bulk annealed
 
Component Elements PropertiesMetricEnglishComments
Al2O3 15.2 %15.2 %
BaO 8.0 %8.0 %
CaO 17.2 %17.2 %
MgO 4.7 %4.7 %
NaO2 0.60 %0.60 %
SiO2 54.3 %54.3 %
 
Descriptive Properties
Velocity of sound, m/s5330

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.