JIS S55C Steel, Tempered
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Very common grade in Asia.

Key Words: Similar to AISI 1050 and 1055 and DIN CK55.
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³AISI 1055
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 229 - 285229 - 285
Hardness, Rockwell C 20.5 - 29.920.5 - 29.9
Tensile Strength, Ultimate 785 MPa114000 psi
Tensile Strength, Yield 588 MPa85300 psi
Elongation at Break 14 %14 %
Reduction of Area 35 %35 %
Modulus of Elasticity 205 GPa29700 ksiTypical steel
Poissons Ratio 0.290.29Typical steel
Machinability 55 %55 %Based on AISI 1212 steel as 100% machinability
Shear Modulus 80.0 GPa11600 ksiTypical steel
Impact 6.06.0kg(f)/cm²
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000163 ohm-cm
@Temperature 0.000 °C
0.0000163 ohm-cm
@Temperature 32.0 °F
condition of specimen unknown
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 20.0 - 100 °C
6.11 µin/in-°F
@Temperature 68.0 - 212 °F
 12.4 µm/m-°C
@Temperature 0.000 - 300 °C
6.89 µin/in-°F
@Temperature 32.0 - 572 °F
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
7.72 µin/in-°F
@Temperature 32.0 - 932 °F
Specific Heat Capacity 0.486 J/g-°C
@Temperature 50.0 - 100 °C
0.116 BTU/lb-°F
@Temperature 122 - 212 °F
(AISI 1045) annealed
Thermal Conductivity 49.8 W/m-K346 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.52 - 0.58 %0.52 - 0.58 %
Chromium, Cr <= 0.20 %<= 0.20 %
Copper, Cu <= 0.30 %<= 0.30 %
Iron, Fe 97.5 - 98.7 %97.5 - 98.7 %
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Nickel, Ni <= 0.20 %<= 0.20 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si 0.15 - 0.35 %0.15 - 0.35 %
Sulfur, S <= 0.035 %<= 0.035 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.