S-Glass Fiber, Generic
Categories: Ceramic; Glass; Glass Fiber; Oxide; Silicon Oxide; Other Engineering Material; Composite Fibers

Material Notes: Used as a reinforcing agent in fiber glass composites, including biomedical/surgical applications.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.48 - 2.49 g/cc0.0896 - 0.0900 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Mohs 6.56.5
Tensile Strength, Ultimate 4585 MPa665000 psiVirgin strength. 50-75% variation in finished product; 8275 MPa at -190°C (-310°F)
 2415 MPa
@Temperature 540 °C
350300 psi
@Temperature 1000 °F
 4445 MPa
@Temperature 370 °C
644700 psi
@Temperature 698 °F
Elongation at Break 5.4 %5.4 %
Modulus of Elasticity 85.5 - 86.9 GPa12400 - 12600 ksi
 88.9 GPa
@Temperature 540 °C
12900 ksi
@Temperature 1000 °F
Poissons Ratio 0.220.22
Shear Modulus 35.0 GPa5080 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 9.05e+10 ohm-cm9.05e+10 ohm-cm
Dielectric Constant  5.1 - 5.34
@Frequency 1e+6 Hz
5.1 - 5.34
@Frequency 1e+6 Hz
 5.0 - 6.4
@Frequency 60 Hz
5.0 - 6.4
@Frequency 60 Hz
Dielectric Strength 13.0 kV/mm330 kV/in
Dissipation Factor  0.0034
@Frequency 1e+6 Hz
0.0034
@Frequency 1e+6 Hz
 0.0129
@Frequency 60 Hz
0.0129
@Frequency 60 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear 5.20 - 5.60 µm/m-°C
@Temperature 20.0 °C
2.89 - 3.11 µin/in-°F
@Temperature 68.0 °F
Specific Heat Capacity 0.737 J/g-°C0.176 BTU/lb-°F
Melting Point <= 1725 °C<= 3137 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5251.525
 
Component Elements PropertiesMetricEnglishComments
Al2O3 24.8 %24.8 %
B2O3 0.010 %0.010 %
BaO 0.20 %0.20 %
CaO 0.010 %0.010 %
FeO 0.21 %0.21 %
MgO 10.27 %10.27 %
NaO2 0.27 %0.27 %
Other 0.030 %0.030 %
SiO2 64.2 %64.2 %
 
Descriptive Properties
Velocity of sound, m/s5850

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.