AISI Type 316L Stainless Steel, annealed sheet
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Similar to Type 316 for superior corrosion resistance, but also has superior resistance to intergranular corrosion following welding or stress relieving. Good corrosion resistance to most chemicals, salts, and acids and molybdenum content helps resistance to marine environments. The low carbon content of 316L reduces the possibility of in vivo corrosion for medical implant use. High creep strength at elevated temperatures. 316L has fabrication characteristics similar to Types 302 and 304.

Applications: biomedical implants, chemical processing, food processing, photographic, pharmaceutical, textile finishing, marine exterior trim.

Key Words: UNS S31603, AISI 316L, ISO 2604-1 F59, ISO 2604-4 P57, ISO 2604-4 P58, ISO 4954 X2CrNiMo17133E, ISO 683/13 19, ISO 683/13 19a, biomaterials, biomedical implants, biocompatible materials
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 7979
Tensile Strength, Ultimate 560 MPa81200 psi
Tensile Strength, Yield 290 MPa42100 psi
Elongation at Break 50 %50 %in 50 mm
Tensile Modulus 193 GPa28000 ksi
Izod Impact  150 J
@Temperature -195 °C
111 ft-lb
@Temperature -319 °F
 150 J
@Temperature 21.0 °C
111 ft-lb
@Temperature 69.8 °F
Charpy Impact 103 J76.0 ft-lbV-notch, 30ºC
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000740 ohm-cm0.0000740 ohm-cmat 20ºC
Magnetic Permeability 1.0081.008at RT
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.500 J/g-°C
@Temperature 0.000 - 100 °C
0.120 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 14.0 - 15.9 W/m-K97.0 - 110 BTU-in/hr-ft²-°F
Melting Point 1375 - 1400 °C2507 - 2550 °F
Solidus 1375 °C2507 °F
Liquidus 1400 °C2550 °F
Maximum Service Temperature, Air 870 °C1600 °FIntermittent
 925 °C1700 °FContinuous Service
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 16 - 18 %16 - 18 %
Iron, Fe 61.9 - 72 %61.9 - 72 %As Balance
Manganese, Mn <= 2.0 %<= 2.0 %
Molybdenum, Mo 2.0 - 3.0 %2.0 - 3.0 %
Nickel, Ni 10 - 14 %10 - 14 %
Phosphorus, P <= 0.045 %<= 0.045 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.