MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Overview of materials for Nylon 66/6, 30% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, 30% Glass Fiber Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66/6, 30% Glass Fiber Reinforced". Specific grades with glass content between 25% and 34% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.23 - 1.62 g/ccAverage value: 1.39 g/cc Grade Count:113
Filler Content 25.0 - 33.0 %Average value: 30.3 % Grade Count:12
Water Absorption 0.500 - 7.00 %Average value: 2.83 % Grade Count:73
Moisture Absorption at Equilibrium 1.00 - 2.50 %Average value: 1.81 % Grade Count:31
 1.40 - 1.90 %
@Temperature 70.0 - 70.0 °C
Average value: 1.65 % Grade Count:4
Water Absorption at Saturation 3.50 - 6.50 %Average value: 4.99 % Grade Count:37
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cmAverage value: 0.00445 cm/cm Grade Count:78
Linear Mold Shrinkage, Transverse 0.00100 - 0.0150 cm/cmAverage value: 0.00670 cm/cm Grade Count:69
Melt Flow 2.00 - 45.0 g/10 minAverage value: 12.4 g/10 min Grade Count:5
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 80.0 - 270 MPaAverage value: 184 MPa Grade Count:46
Tensile Strength, Ultimate 45.0 - 200 MPaAverage value: 137 MPa Grade Count:107
Tensile Strength, Yield 70.0 - 180 MPaAverage value: 117 MPa Grade Count:14
Elongation at Break 1.80 - 35.0 %Average value: 4.27 % Grade Count:108
Elongation at Yield 3.00 - 6.00 %Average value: 4.29 % Grade Count:12
Modulus of Elasticity 1.80 - 99.4 GPaAverage value: 8.85 GPa Grade Count:91
Flexural Yield Strength 56.0 - 275 MPaAverage value: 200 MPa Grade Count:46
Flexural Modulus 3.70 - 10.5 GPaAverage value: 7.74 GPa Grade Count:48
Poissons Ratio 0.330 - 0.400Average value: 0.352 Grade Count:13
Izod Impact, Notched 0.550 - 1.50 J/cmAverage value: 1.13 J/cm Grade Count:7
Izod Impact, Notched (ISO) 4.00 - 21.0 kJ/m²Average value: 11.6 kJ/m² Grade Count:25
 7.20 - 11.0 kJ/m²
@Temperature -40.0 - -30.0 °C
Average value: 8.48 kJ/m² Grade Count:3
Charpy Impact Unnotched 2.50 J/cm² - NBAverage value: 6.44 J/cm² Grade Count:89
 2.40 J/cm² - NB
@Temperature -40.0 - -20.0 °C
Average value: 5.14 J/cm² Grade Count:74
Charpy Impact, Notched 0.399 - 8.50 J/cm²Average value: 1.22 J/cm² Grade Count:96
 0.200 - 5.50 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 0.856 J/cm² Grade Count:72
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+9 - 1.00e+15 ohm-cmAverage value: 1.72e+14 ohm-cm Grade Count:63
Surface Resistance 1.00e+10 - 1.00e+15 ohmAverage value: 1.29e+14 ohm Grade Count:43
Dielectric Constant 3.00 - 4.30Average value: 3.69 Grade Count:6
Dielectric Strength 12.0 - 60.0 kV/mmAverage value: 30.2 kV/mm Grade Count:55
Dissipation Factor 0.00500 - 0.100Average value: 0.0206 Grade Count:11
Arc Resistance 60.0 - 120 secAverage value: 90.0 sec Grade Count:4
Comparative Tracking Index 175 - 650 VAverage value: 534 V Grade Count:53
Hot Wire Ignition, HWI 120 secAverage value: 120 sec Grade Count:7
High Amp Arc Ignition, HAI 120 arcsAverage value: 120 arcs Grade Count:7
High Voltage Arc-Tracking Rate, HVTR 80.0 - 150 mm/minAverage value: 115 mm/min Grade Count:4
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.0 - 80.0 µm/m-°CAverage value: 24.1 µm/m-°C Grade Count:44
 10.0 - 20.0 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 17.2 µm/m-°C Grade Count:6
 20.0 - 20.0 µm/m-°C
@Temperature 35.0 - 55.0 °C
Average value: 17.2 µm/m-°C Grade Count:2
 20.0 - 20.0 µm/m-°C
@Thickness 2.00 - 2.00 mm
Average value: 17.2 µm/m-°C Grade Count:2
CTE, linear, Transverse to Flow 45.0 - 110 µm/m-°CAverage value: 75.0 µm/m-°C Grade Count:43
 91.0 - 130 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 109 µm/m-°C Grade Count:6
Specific Heat Capacity 2.00 - 2.00 J/g-°C
@Temperature 280 - 280 °C
Average value: 2.00 J/g-°C Grade Count:1
Thermal Conductivity 0.250 - 0.250 W/m-K
@Temperature 280 - 280 °C
Average value: 0.250 W/m-K Grade Count:1
Melting Point 200 - 312 °CAverage value: 263 °C Grade Count:82
Maximum Service Temperature, Air 90.0 - 270 °CAverage value: 173 °C Grade Count:42
Deflection Temperature at 0.46 MPa (66 psi) 215 - 300 °CAverage value: 246 °C Grade Count:21
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 285 °CAverage value: 222 °C Grade Count:90
Deflection Temperature at 8.0 MPa 50.0 - 204 °CAverage value: 139 °C Grade Count:35
Vicat Softening Point 195 - 252 °CAverage value: 226 °C Grade Count:5
Glass Transition Temp, Tg 45.0 - 90.0 °CAverage value: 67.5 °C Grade Count:4
UL RTI, Electrical 65.0 - 160 °CAverage value: 113 °C Grade Count:11
UL RTI, Mechanical with Impact 65.0 - 105 °CAverage value: 75.9 °C Grade Count:7
UL RTI, Mechanical without Impact 65.0 - 140 °CAverage value: 88.2 °C Grade Count:7
Flammability, UL94 HB - 5VAGrade Count:65
 HB - HB
@Temperature 1.50 - 1.50 °C
Grade Count:1
Flame Spread 80.0 mm/minAverage value: 80.0 mm/min Grade Count:3
Oxygen Index 23.0 - 42.0 %Average value: 34.5 % Grade Count:12
Glow Wire Test 650 - 960 °CAverage value: 850 °C Grade Count:18
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 240 - 304 °CAverage value: 271 °C Grade Count:8
Melt Temperature 225 - 330 °CAverage value: 277 °C Grade Count:28
Mold Temperature 60.0 - 130 °CAverage value: 91.4 °C Grade Count:29
Drying Temperature 79.4 - 100 °CAverage value: 83.4 °C Grade Count:26
Moisture Content 0.0500 - 0.200 %Average value: 0.158 % Grade Count:20
Injection Pressure 34.5 - 138 MPaAverage value: 91.2 MPa Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 30% Glass Fiber Filled
Overview of materials for Nylon 66/6
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Overview of materials for Nylon 66/6, 20% Glass Fiber Reinforced
Overview of materials for Nylon 66/6, 40% Glass Fiber Reinforced

O2493 / 77994

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.