MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI adhesives

(Viewing data as-entered. Click here to return)
Eastman Eastar MN052 Polyester, Natural
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Eastar™ Polyester MN052 has been tested for FDA/ISO 10993 and USP Class VI Biological Evaluation testing after Gamma and EtO sterilization. Eastar™ Polyester MN052 does not contain a mold release. It has a relatively high flex modulus and yield strength. This product has high flow characteristics. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED

Applications/Uses:

  • Drug Delivery
  • Labware
  • Medical
Key Attributes:
  • Chemical resistance to most medical solvents including lipids and IPA
  • Gamma and E-beam color stability

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.32 g/ccASTM D792
Water Absorption 0.10 %24h Immersion; ASTM D570
Linear Mold Shrinkage 0.0040 cm/cm
@Thickness 3.20 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 110ASTM D785
Tensile Strength at Break 26.0 MPaASTM D638
Tensile Strength, Yield 57.0 MPaASTM D638
Elongation at Yield 4.0 %ASTM D638
Flexural Yield Strength 81.0 MPaASTM D790
Flexural Modulus 2.50 GPaASTM D790
Izod Impact, Notched 0.360 J/cm
@Temperature -40.0 °C
ASTM D256
 51.0 J/m
@Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched NBASTM D4812
 NB
@Temperature -40.0 °C
ASTM D4812
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmASTM D257
Surface Resistivity per Square 1.00e+16 ohmASTM D257
Dielectric Constant 3.0
@Frequency 1e+6 Hz
ASTM D150
 3.2
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 15.7 kV/mmShort Time, 500V/sec; ASTM D149
Dissipation Factor 0.0080
@Frequency 1000 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 155 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 66.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °CASTM D648
Vicat Softening Point 79.0 °C1kg load; ASTM D1525
 
Processing PropertiesOriginal ValueComments
Melt Temperature 275 - 295 °C
Mold Temperature 10.0 - 30.0 °C
Drying Temperature 150 - 160 °C
Dry Time 4 - 6 hour
 
Compliance PropertiesOriginal ValueComments
USP Class VI Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman 7352 PET
BASF Ultrason® S 2010 PSU
BASF Ultrason® E 2010 PES
BASF Ultramid® C3U10 PA6/66 FR (Dry)
BASF Ultramid® B3WG6 30% Glass Filled PA6 (Dry)

PE9061 / 35117

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.