MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Parker Chomerics THERM-A-FORM T642 Cure-in-Place Potting and Underfill Material
Categories: Polymer; Thermoset; Silicone

Material Notes: Description: THERM-A-FORM™ thermally conductive silicone elastomer products are dispensable form-in-place compounds designed for heat transfer without excessive compressive force in electronics cooling applications. These versatile liquid reactive materials can be dispensed and cured into complex geometries for cooling of multi-height components on a PCB without the expense of a molded sheet. Each compound is available in ready-to-use cartridge systems, eliminating weighing, mixing, and degassing procedures.

Product Attributes: High thermal performance with flexibility; ideal for underfilling and low outgassing

Information provided by Chomerics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.50 g/ccASTM D792
Viscosity 2.5 cPASTM D2196
Outgassing - Total Mass Loss 0.32 %TML; ASTM D595
Collected Volatile Condensable Material 0.21 %ASTM D595
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70ASTM D2240
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmASTM D257
Dielectric Constant 4.0
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 20.0 kV/mmASTM D149
Dissipation Factor 0.0010
@Frequency 1e+6 Hz
Chomerics
 
Thermal PropertiesOriginal ValueComments
CTE, linear 300 µm/m-°CASTM E831
Specific Heat Capacity 1.00 J/g-°CASTM E1269
Thermal Conductivity 1.20 W/m-KASTM D5470
Maximum Service Temperature, Air 150 °C
Minimum Service Temperature, Air -50.0 °C
Brittleness Temperature -75.0 °CASTM D2137
 
Processing PropertiesOriginal ValueComments
Cure Time 0.0500 hour
@Temperature 150 °C
 0.500 hour
@Temperature 70.0 °C
 48.0 hour
@Temperature 23.0 °C
Pot Life 60.0 min
@Temperature 23.0 °C
2X Starting Viscosity
Shelf Life 3.00 MonthFrom date of Manufacture
 
Descriptive Properties
BinderSilicone
ColorBlue
FillerBoron Nitride
Mix Ratio10:1
Number of Components2-part

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow SE 738 SILICONE RTV
Dow SE 4486 SILICONE RTV
Dow SE 4422 SILICONE RTV
Dow 3-4680 SILICONE GEL KIT
Dow 3120 RTV SILICONE RUBBER

PCHOME426 / 131136

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.