MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

Magnesium Elektron Elektron® MSR-B Magnesium Casting Alloy, UNS M18220
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: ELEKTRON MSR-B is a high strength magnesium casting alloy developed by Magnesium Elektron to have good ambient and elevated temperature properties whilst retaining good foundry characteristics. It is a fully heat treatable magnesium alloy containing silver and rare earth metals. It is pressure tight, weldable and may be used up to temperatures of 200°C.

Applications: The alloys will be of interest to designers requiring good retention of properties at elevated temperatures for aerospace, automotive and military applications.

Information provided by Magnesium Elektron.

Key Words: AECMA MG-C-51; AFNOR G-Ag2.5TR; MOD DTD 5035A; UNS M18220; ISO 16220 MC65210
Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.82 g/cc1.82 g/cc
Bulk Density 1.82 g/cc0.0658 lb/in³Value supplied by MatWeb
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 80 - 10580 - 105
Tensile Strength at Break >= 240 MPa>= 34800 psiMin Design Specification
 160 MPa
@Temperature 250 °C
23200 psi
@Temperature 482 °F
 185 MPa
@Temperature 200 °C
26800 psi
@Temperature 392 °F
 208 MPa
@Temperature 150 °C
30200 psi
@Temperature 302 °F
 230 MPa
@Temperature 100 °C
33400 psi
@Temperature 212 °F
 266 MPa
@Temperature 22.0 °C
38600 psi
@Temperature 71.6 °F
Tensile Strength, Yield >= 185 MPa
@Strain 0.2 %
>= 26800 psi
@Strain 0.2 %
Min Design Specification
 122 MPa
@Strain 0.2 %,
Temperature 250 °C
17700 psi
@Strain 0.2 %,
Temperature 482 °F
 165 MPa
@Strain 0.2 %,
Temperature 200 °C
23900 psi
@Strain 0.2 %,
Temperature 392 °F
 182 MPa
@Strain 0.2 %,
Temperature 150 °C
26400 psi
@Strain 0.2 %,
Temperature 302 °F
 195 MPa
@Strain 0.2 %,
Temperature 100 °C
28300 psi
@Strain 0.2 %,
Temperature 212 °F
 205 MPa
@Strain 0.2 %,
Temperature 22.0 °C
29700 psi
@Strain 0.2 %,
Temperature 71.6 °F
Elongation at Break >= 2.0 %>= 2.0 %Min Design Specification
 4.0 %
@Temperature 22.0 °C
4.0 %
@Temperature 71.6 °F
in 5.65 A½
 15 %
@Temperature 100 °C
15 %
@Temperature 212 °F
 19 %
@Temperature 150 °C
19 %
@Temperature 302 °F
 24 %
@Temperature 200 °C
24 %
@Temperature 392 °F
 30 %
@Temperature 250 °C
30 %
@Temperature 482 °F
Creep Strength  10.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
1450 psi
@Temperature 482 °F,
Time 1000 hour
0.1% creep
 14.0 MPa
@Temperature 250 °C,
Time 1.80e+6 sec
2030 psi
@Temperature 482 °F,
Time 500 hour
0.1% creep
 16.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
2320 psi
@Temperature 482 °F,
Time 1000 hour
0.2% creep
 21.0 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
3050 psi
@Temperature 482 °F,
Time 1000 hour
0.3% creep
 22.0 MPa
@Temperature 250 °C,
Time 1.80e+6 sec
3190 psi
@Temperature 482 °F,
Time 500 hour
0.2% creep
 26.0 MPa
@Temperature 250 °C,
Time 360000 sec
3770 psi
@Temperature 482 °F,
Time 100 hour
0.1% creep
 27.0 MPa
@Temperature 250 °C,
Time 1.80e+6 sec
3920 psi
@Temperature 482 °F,
Time 500 hour
0.3% creep
 34.0 MPa
@Temperature 250 °C,
Time 360000 sec
4930 psi
@Temperature 482 °F,
Time 100 hour
0.2% creep
 41.0 MPa
@Temperature 250 °C,
Time 360000 sec
5950 psi
@Temperature 482 °F,
Time 100 hour
0.3% creep
 43.0 MPa
@Temperature 250 °C,
Time 36000 sec
6240 psi
@Temperature 482 °F,
Time 10.0 hour
0.1% creep
 46.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
6670 psi
@Temperature 392 °F,
Time 1000 hour
0.1% creep
 54.0 MPa
@Temperature 200 °C,
Time 1.80e+6 sec
7830 psi
@Temperature 392 °F,
Time 500 hour
0.1% creep
 56.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
8120 psi
@Temperature 392 °F,
Time 1000 hour
0.2% creep
 65.0 MPa
@Temperature 200 °C,
Time 1.80e+6 sec
9430 psi
@Temperature 392 °F,
Time 500 hour
0.2% creep
 72.0 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
10400 psi
@Temperature 392 °F,
Time 1000 hour
0.3% creep
 74.0 MPa
@Temperature 200 °C,
Time 360000 sec
10700 psi
@Temperature 392 °F,
Time 100 hour
0.1% creep
 83.0 MPa
@Temperature 200 °C,
Time 1.80e+6 sec
12000 psi
@Temperature 392 °F,
Time 500 hour
0.3% creep
 86.0 MPa
@Temperature 200 °C,
Time 360000 sec
12500 psi
@Temperature 392 °F,
Time 100 hour
0.2% creep
 102 MPa
@Temperature 200 °C,
Time 36000 sec
14800 psi
@Temperature 392 °F,
Time 10.0 hour
0.1% creep
 103 MPa
@Temperature 200 °C,
Time 360000 sec
14900 psi
@Temperature 392 °F,
Time 100 hour
0.3% creep
 123 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
17800 psi
@Temperature 302 °F,
Time 1000 hour
0.2% creep
 135 MPa
@Temperature 150 °C,
Time 1.80e+6 sec
19600 psi
@Temperature 302 °F,
Time 500 hour
0.2% creep
 151 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
21900 psi
@Temperature 302 °F,
Time 1000 hour
0.3% creep
 160 MPa
@Temperature 150 °C,
Time 1.80e+6 sec
23200 psi
@Temperature 302 °F,
Time 500 hour
0.3% creep
Modulus of Elasticity 44.1 GPa6400 ksi
Compressive Yield Strength 165 - 200 MPa
@Strain 0.2 %
23900 - 29000 psi
@Strain 0.2 %
Compressive Strength 310 - 385 MPa45000 - 55800 psi
Poissons Ratio 0.300.30
Fatigue Strength 100 - 110 MPa
@# of Cycles 5.00e+7
14500 - 16000 psi
@# of Cycles 5.00e+7
Rotating Bend, Unnotched
Fracture Toughness 14.9 MPa-m½13.6 ksi-in½KIC
Shear Strength 152 MPa22000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000680 ohm-cm0.00000680 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 26.7 µm/m-°C14.8 µin/in-°F
Specific Heat Capacity 1.00 J/g-°C0.239 BTU/lb-°F
Thermal Conductivity 113 W/m-K784 BTU-in/hr-ft²-°F
Melting Point 550 - 640 °C1020 - 1180 °F
Solidus 550 °C1020 °F
Liquidus 640 °C1180 °F
Shrinkage 1.3 %1.3 %Pattern Makers Shrinkage Factor
 
Component Elements PropertiesMetricEnglishComments
Magnesium, Mg 93 - 95.6 %93 - 95.6 %As Balance
Rare Earths 2.0 - 3.0 %2.0 - 3.0 %
Silver, Ag 2.0 - 3.0 %2.0 - 3.0 %
Zirconium, Zr 0.40 - 1.0 %0.40 - 1.0 %
 
Descriptive Properties
Corrosion rate430 mpyASTM B117 Salt spray test
Damping Index0.4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Magnesium Elektron Elektron® 43 Magnesium Wrought Alloy
Magnesium Elektron Elektron® QE22 Magnesium Casting Alloy, UNS M18220
Magnesium Elektron Elektron® RZ5 Magnesium Casting Alloy, UNS M16410
Magnesium Elektron Elektron® 21 Magnesium Casting Alloy
Magnesium Elektron Elektron® WE43B Magnesium Casting Alloy, UNS M18430

NMAGEL903 / 186918

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.