MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

EMS-Grivory Grilon® BM-30 PA6-MD30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Mineral Filled

Material Notes: Product description: Grilon BM-30 is a 30% mineral reinforced PA6 injection moulding grade. Grilon BM-30 has the following important properties:
  • heat stabilized
  • impact resistant
  • isotropic shrinkage
  • light inherent colour
Application examples are engineering parts with high stiffness and low warpage properties.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.38 g/cc0.0499 lb/in³Dry; ISO 1183
Water Absorption 7.0 %7.0 %Sim. to ISO 62
Moisture Absorption 1.80 %1.80 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0080 cm/cm0.0080 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 70.0 MPa10200 psiConditioned; ISO 2039-1
 170 MPa24700 psiDry; ISO 2039-1
Tensile Strength at Break 40.0 MPa5800 psiConditioned; ISO 527-1/-2
 90.0 MPa13100 psiDry; ISO 527-1/-2
Elongation at Break 3.0 %3.0 %Dry; ISO 527-1/-2
 40 %40 %Conditioned; ISO 527-1/-2
Tensile Modulus 3.00 GPa435 ksiConditioned; ISO 527-1/-2
 6.50 GPa943 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  4.50 J/cm²
@Temperature 23.0 °C
21.4 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
 4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  0.200 J/cm²
@Temperature -30.0 °C
0.952 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.200 J/cm²
@Temperature -30.0 °C
0.952 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 222 °C432 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 100 - 120 °C212 - 248 °FLong Term; ISO 2578
 180 °C356 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 100 °C212 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveInterior
FormGranules
Industry & Consumer goodsMechanical Engineering
 Tools & Accessories
ProcessingInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Minlon® 73M40 NC010 PA6-MD40
Envalior Durethan® BM 230 H2.0 901510 Nylon 6 (PA6), 30% Mineral Filled, Dry
Eastman Tenite 264-10 CAB Cellulose Acetate Butyrate
EMS-Grivory Grilon® AG-30 H PA66
Eastman Tenite 264-16 CAB Cellulose Acetate Butyrate

PGRH204 / 156913

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.