MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Alclad Aluminum 2219-T37
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Key Words: UNS A82219
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.84 g/cc0.103 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  >= 310 MPa
@Thickness 1.02 - 2.51 mm
>= 45000 psi
@Thickness 0.0400 - 0.0990 in
Sheet and plate
 >= 325 MPa
@Thickness 2.54 - 12.7 mm
>= 47100 psi
@Thickness 0.100 - 0.499 in
Sheet and plate
Tensile Strength, Yield  >= 235 MPa
@Thickness 1.02 - 2.51 mm
>= 34100 psi
@Thickness 0.0400 - 0.0990 in
Sheet and plate
 >= 240 MPa
@Thickness 2.54 - 12.7 mm
>= 34800 psi
@Thickness 0.100 - 0.499 in
Sheet and plate
Elongation at Break  6.0 %
@Thickness 1.02 - 2.51 mm
6.0 %
@Thickness 0.0400 - 0.0990 in
Sheet and plate
 6.0 %
@Thickness 2.54 - 12.7 mm
6.0 %
@Thickness 0.100 - 0.499 in
Sheet and plate
Modulus of Elasticity 73.8 GPa10700 ksi
Compressive Modulus 75.2 GPa10900 ksi
Poissons Ratio <= 0.33<= 0.33
Shear Modulus 27.7 GPa4020 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000620 ohm-cm0.00000620 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.6 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
12.5 µin/in-°F
@Temperature 68.0 - 212 °F
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.0 µin/in-°F
@Temperature 68.0 - 392 °F
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
13.6 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.864 J/g-°C0.207 BTU/lb-°F
Thermal Conductivity 116 W/m-K805 BTU-in/hr-ft²-°F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 97.55 - 99.2 %97.55 - 99.2 %
Copper, Cu <= 0.10 %<= 0.10 %
Magnesium, Mg <= 0.10 %<= 0.10 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.050 %<= 0.050 %
Other, total <= 0.15 %<= 0.15 %
Si+Fe <= 0.70 %<= 0.70 %
Zinc, Zn 0.80 - 1.3 %0.80 - 1.3 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Alclad Aluminum 2219-T62
Alclad Aluminum 2219-T31
Aluminum 2219-T81
Aluminum 7075-T6; 7075-T651
Alclad Aluminum 2219-T351

MA2219AT37 / 109173

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.