MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

EMS-Grivory Grilon® EBGM-30 HX PA666-GF30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, 30% Glass Fiber Reinforced

Material Notes: Product description: Grilon EBGM-30 HX is a specially heat stabilized PA66+PA6 injection molding grade with 30% glass fibers. Grilon EBGM-30 HX has the following important properties:
  • High heat resistance
  • High stiffness
  • Good flowability
  • Good welding behavior
Application examples: Grilon EBGM-30 HZ is especially suitable for production of technical parts in the application fields of:
    Charged air ducts
  • Connectors for air ducts
  • Applications under the bonnet
  • All applications with high heat resistance.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.37 g/cc0.0495 lb/in³Dry; ISO 1183
Water Absorption 5.5 %5.5 %Sim. to ISO 62
Moisture Absorption 2.00 %2.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 105 MPa15200 psiConditioned; ISO 2039-1
 210 MPa30500 psiDry; ISO 2039-1
Tensile Strength at Break 90.0 MPa13100 psiConditioned; ISO 527-1/-2
 155 MPa22500 psiDry; ISO 527-1/-2
Elongation at Break 3.0 %3.0 %Dry; ISO 527-1/-2
 6.0 %6.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 5.50 GPa798 ksiConditioned; ISO 527-1/-2
 9.50 GPa1380 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  6.50 J/cm²
@Temperature -30.0 °C
30.9 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 6.50 J/cm²
@Temperature -30.0 °C
30.9 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 7.00 J/cm²
@Temperature 23.0 °C
33.3 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
 7.00 J/cm²
@Temperature 23.0 °C
33.3 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 1.10 J/cm²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+9 ohm-cm1.00e+9 ohm-cmConditioned; IEC 60093
 1.00e+10 ohm-cm1.00e+10 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 34.0 kV/mm864 kV/inConditioned; IEC 60243-1
 38.0 kV/mm965 kV/inDry; IEC 60243-1
Comparative Tracking Index 500 V500 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C11.1 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C44.4 µin/in-°FISO 11359-1/-2
Melting Point 260 °C500 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 130 - 150 °C266 - 302 °FLong Term; ISO 2578
 230 °C446 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 225 °C437 °FISO 75-1/-2
Deflection Temperature at 8.0 MPa 155 °C311 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveAir intake systems
FormGranules
ProcessingExtrusion - blow molding
 Injection Molding
 Other Extrusion
Product AttributesNanocomposite
Special CharacteristicsImproved heat resistance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® C3 GF 30 5 XTC (4499) PA66/6 Dry, 30% Glass Filled
LG Chemical LUMID GP2301BF PA 66+GF30%, Flame Retardant
Akro-Plastic Akromid® C3 GF 30 5 XTC (4499) PA66/6 Conditioned, 30% Glass Filled
Akro-Plastic Akromid® C3 GF 30 1 black (4363) PA 6.6/6 Dry, Heat Stabilized
DuPont Mobility and Materials Zytel® HTN 55G55LWSF BK752A Polyphthalamide (PPA)

PGRH232 / 156941

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.