MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ATI Allegheny Ludlum 309H Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes:

Characteristics: comparable corrosion resistance, superior resistance to oxidation, and the retention of a larger fraction of room temperature strength than common austenitic alloys. Good creep deformation resistance.

Applications:Heat treatment industry-conveyor belts, rollers, burner parts, refractory supports, retorts linings, oven linings, fans, tube hangers, baskets, and trays. Chemical process industry- containers for hot concentrated acids, ammonia, and sulfur dioxide. Food processing industry- used in contact with hot acetic and citric acid.

Information provided by Allegheny Ludlum

Key Words: UNS S30909
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.03 g/cc0.290 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Creep Strength  24.0 MPa
@Temperature 788 °C,
Time 3.60e+7 sec
3480 psi
@Temperature 1450 °F,
Time 10000 hour
1% creep
 83.0 MPa
@Temperature 593 °C,
Time 3.60e+7 sec
12000 psi
@Temperature 1100 °F,
Time 10000 hour
1% creep
Rupture Strength  17.0 MPa
@Temperature 899 °C,
Time 3.60e+7 sec
2470 psi
@Temperature 1650 °F,
Time 10000 hour
 83.0 MPa
@Temperature 677 °C,
Time 3.60e+7 sec
12000 psi
@Temperature 1250 °F,
Time 10000 hour
Modulus of Elasticity 200 GPa29000 ksi
Poissons Ratio 0.300.30calculated
Shear Modulus 77.0 GPa11200 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000780 ohm-cm
@Temperature 20.0 °C
0.0000780 ohm-cm
@Temperature 68.0 °F
 0.0001148 ohm-cm
@Temperature 1200 °C
0.0001148 ohm-cm
@Temperature 2190 °F
Magnetic Permeability 1.021.02at 200H
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.6 µm/m-°C
@Temperature 20.0 - 100 °C
8.67 µin/in-°F
@Temperature 68.0 - 212 °F
 17.6 µm/m-°C
@Temperature 20.0 - 500 °C
9.78 µin/in-°F
@Temperature 68.0 - 932 °F
 19.4 µm/m-°C
@Temperature 20.0 - 1000 °C
10.8 µin/in-°F
@Temperature 68.0 - 1830 °F
Specific Heat Capacity 0.502 J/g-°C
@Temperature 0.000 - 100 °C
0.120 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  15.6 W/m-K
@Temperature 20.0 - 100 °C
108 BTU-in/hr-ft²-°F
@Temperature 68.0 - 212 °F
 18.7 W/m-K
@Temperature 20.0 - 500 °C
130 BTU-in/hr-ft²-°F
@Temperature 68.0 - 932 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.040 - 0.10 %0.040 - 0.10 %
Chromium, Cr 22 - 24 %22 - 24 %
Iron, Fe 58.075 - 63.135 %58.075 - 63.135 %As Remainder
Manganese, Mn 2.0 %2.0 %
Nickel, Ni 12 - 15 %12 - 15 %
Phosphorus, P 0.045 %0.045 %
Silicon, Si 0.75 %0.75 %
Sulfur, S 0.030 %0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NL1002 / 17770

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.