MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Lubrizol ESTANE® GP85AE Ester Based Thermoplastic Polyurethane
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Type: Estane® GP 85AE is an aromatic polyester-based thermoplastic polyurethane (TPU).

Appearance: Translucent spherical pellets

Uses: Injection molding parts

Available in Europe

Information provided by Lubrizol.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.23 g/cc1.23 g/ccISO 2781
Maximum Moisture Content 0.0500.050
Melt Flow 10 - 35 g/10 min
@Load 8.70 kg,
Temperature 195 °C
10 - 35 g/10 min
@Load 19.2 lb,
Temperature 383 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8585ISO 868
Hardness, Shore D 3737ISO 868
Tensile Strength, Ultimate 38.0 MPa5510 psiISO 37
Elongation at Break 680 %680 %ISO 37
Tensile Modulus 0.0150 GPa2.18 ksiISO 527
50% Modulus 4.50 MPa
@Strain 50 %
4.50 MPa
@Strain 50 %
ISO 37
100% Modulus 6.00 MPa
@Strain 100 %
870 psi
@Strain 100 %
ISO 37
300% Modulus 10.5 MPa
@Strain 300 %
1520 psi
@Strain 300 %
ISO 37
Rebound 41 %41 %ISO 4662
Tear Strength 67.0 kN/m382 pliwith incision; ISO 34B
 100 kN/m571 pliwithout incision; ISO 34B
Abrasion 3030mm3; ISO 4649
Compression Set  24 %
@Temperature 22.0 °C,
Time 252000 sec
24 %
@Temperature 71.6 °F,
Time 70.0 hour
ISO 815
 38 %
@Temperature 70.0 °C,
Time 86400 sec
38 %
@Temperature 158 °F,
Time 24.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 105 °C221 °FA50; ISO 306
 
Processing PropertiesMetricEnglishComments
Feed Temperature 40.0 °C104 °FInjection
Nozzle Temperature 190 - 200 °C374 - 392 °FInjection
Zone 1 185 - 195 °C365 - 383 °FInjection
Zone 2 190 - 200 °C374 - 392 °FInjection
Zone 3 195 - 205 °C383 - 401 °FInjection
Zone 4 195 - 205 °C383 - 401 °FInjection
Drying Temperature 90.0 °C194 °F
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hour
Dew Point -30.0 °C-22.0 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hytrel® HTR8351 NC021 TPC-ET
Envalior Arnitel® EM400 TPC-ET, Injection Molding or Extrusion Grade
Austin Novel Materials Texalan® 598A Polyether-based TPU
Austin Novel Materials Texalan® 590A Polyether-based TPU
Austin Novel Materials Texalan® 498A Polyester-based TPU

PNOVEON159 / 55428

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.