Lubrizol Estane® ZHF 90AT2 Thermoplastic Polyurethane
Categories:
Polymer
;
Thermoplastic
;
Polyurethane, TP
Material Notes:
Type: Estane® ZHF 90AT2 is a non-halogen, flame retardant, aromatic polyether-based thermoplastic polyurethane.
Application: Extrusion
Information provided by The 159 Corporation
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.24
g/cc
1.24
g/cc
ISO 2781
Maximum Moisture Content
0.020
0.020
Mechanical Properties
Metric
English
Comments
Hardness, Shore A
88
88
ISO 868
Tensile Strength
28.0
MPa
4060
psi
ISO 527-2/5A/200
Elongation at Break
520 %
520 %
ISO 527-2/5A/200
50% Modulus
8.00
MPa
@Strain 50 %
8.00
MPa
@Strain 50 %
ISO 527-2/5A/200
100% Modulus
10.0
MPa
@Strain 100 %
1450
psi
@Strain 100 %
ISO 527-2/5A/200
300% Modulus
14.0
MPa
@Strain 300 %
2030
psi
@Strain 300 %
ISO 527-2/5A/200
Tear Strength
85.0
kN/m
485
pli
Nicked; ISO 34-1B
Abrasion
90
90
[mm3]; ISO 4649-B
Thermal Properties
Metric
English
Comments
Vicat Softening Point
85.0
°C
185
°F
A50; ISO 306
Flammability, UL94
V-2
@Thickness 3.00 mm
V-2
@Thickness 0.118 in
Smoke Density
38
@Thickness 0.750 mm
38
@Thickness 0.0295 in
Flaming DM; ASTM E662
112
@Thickness 0.750 mm
112
@Thickness 0.0295 in
Non flaming DM; ASTM E662
Processing Properties
Metric
English
Comments
Zone 1
200
°C
392
°F
Zone 2
205
°C
401
°F
Zone 3
210
°C
410
°F
Zone 4
205
°C
401
°F
Adapter Temperature
205
°C
401
°F
5
Die Temperature
200
°C
392
°F
Tip
205
°C
401
°F
Drying Temperature
82.0
°C
@Time 7200 - 14400 sec
180
°F
@Time 2.00 - 4.00 hour
Dew Point
-40.0
°C
-40.0
°F
Component Elements Properties
Metric
English
Comments
Loss on Ignition(%)
24 %
24 %
ASTM D-2863
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PLUBR5028 / 238898
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.