MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL PPX™ Resin PPX630 Polyphenylene Ether + PP (PPE+PP) (Europe)
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polypropylene (PP)

Material Notes: NORYL PPX™ 630 resin is a 30% glass reinforced alloy of polyphenylene ether (PPE) + polypropylene (PP). This injection moldable grade exhibits high elongation and high stiffness along with temperature performance, impact resistance, hydrolytic and dimensional stability. NORYL PPX630 resin is an excellent candidate for hot water system exteriors, condensate housings, and printer internals. *See NORYL PPX630F resin for NSF 61.

Features: Hydrolytic Stability,Chemical Resistance,Low Creep Sensitivity,Good Stiffness,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.0400 %0.0400 %23°C / 50% RH
Water Absorption at Saturation 0.20 %0.20 %ISO 62-1
Viscosity 3.0 cP
@Load 5.00 kg,
Temperature 260 °C
3.0 cP
@Load 11.0 lb,
Temperature 500 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0020 - 0.0030 cm/cm0.0020 - 0.0030 in/inSABIC method
Linear Mold Shrinkage, Transverse 0.0020 - 0.0070 cm/cm0.0020 - 0.0070 in/inSABIC method
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 75.0 MPa10900 psiH358/30; ISO 2039-1
Tensile Strength at Break 80.0 MPa11600 psi5 mm/min; ISO 527
Elongation at Break 4.1 %4.1 %5 mm/min; ISO 527
Tensile Modulus 6.60 GPa957 ksi1 mm/min; ISO 527
Flexural Strength 120 MPa17400 psibreak, 2mm/min; ISO 178
Flexural Modulus 5.50 GPa798 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO) 15.0 kJ/m²7.14 ft-lb/in²80*10*4; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 48.0 kJ/m²22.8 ft-lb/in²80*10*4; ISO 180/1U
 46.0 kJ/m²
@Temperature -30.0 °C
21.9 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1U
Charpy Impact Unnotched 5.00 J/cm²23.8 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 1.50 J/cm²7.14 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant  2.4
@Frequency 1e+6 Hz
2.4
@Frequency 1e+6 Hz
IEC 60250
 2.4
@Frequency 50.0 - 60.0 Hz
2.4
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 24.0 kV/mm
@Thickness 3.20 mm
610 kV/in
@Thickness 0.126 in
in oil; IEC 60243-1
Dissipation Factor  0.00030
@Frequency 50.0 - 60.0 Hz
0.00030
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.0010
@Frequency 1e+6 Hz
0.0010
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 500 V500 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
11.1 µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
CTE, linear, Transverse to Flow 115 µm/m-°C
@Temperature 23.0 - 60.0 °C
63.9 µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
Hot Ball Pressure Test 125 °C257 °FPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 155 °C311 °FEdgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 135 °C275 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 125 °C257 °FRate B/50; ISO 306
 128 °C262 °FRate B/120; ISO 306
Flammability, UL94 HB
@Thickness >=1.50 mm
HB
@Thickness >=0.0591 in
UL 94
Glow Wire Flammability Index 650 °C
@Thickness 3.20 mm
1200 °F
@Thickness 0.126 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 260 - 300 °C500 - 572 °F
Zone 2 250 - 290 °C482 - 554 °F
Zone 3 255 - 290 °C491 - 554 °F
Melt Temperature 260 - 300 °C500 - 572 °FInjection Molding
Mold Temperature 40.0 - 65.0 °C104 - 149 °F
Drying Temperature 65.0 - 75.0 °C149 - 167 °FInjection Molding
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection Molding
Precipitation Temperature 60.0 - 80.0 °C140 - 176 °FHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82208 / 290155

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.