MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ethydco Advancene™ EE-1801-BSB LLDPE Blown Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Butene, Film

Material Notes: ADVANCENE™ EE-1801-BSB is a part of a Butene LLDPE series offering excellent drawdown and puncture resistance combined with high gloss and clarity. They are also frequently used as a blend partner with LDPE resins to improve film properties and processability. Several additive packages are available according to the required surface properties. Applications: • Agricultural Film. • Bag in Box. • Barrier Food Packaging. • Blown Film. • Bread Bags. • Food Packaging. • Form Fill and Seal Packaging. • Freezer Film. • Garment Film. • General Packaging. • Heavy Duty Bags. • Ice Bags. • Industrial Liners. • Industrial Packaging. • Lamination Film. • Liners. • Multilayer Packaging Film. • Packaging Films. • Produce Bags. • Refuse Bags. • Shoppers. • Stand Up Pouches. • Trash Bags.

Processing Notes: The film properties have been measured on 30 µm (1.18 mil) thick films (Blow-up ratio : 2.5).

Information provided by ETHYDCO.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.918 g/ccASTM D792
Melt Index of Compound 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238, ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 590 %ASTM D882
Film Elongation at Break, TD 860 %ASTM D882
Elmendorf Tear Strength MD 120 gASTM 1922, ISO 6383-2
Elmendorf Tear Strength TD 480 gASTM 1922, ISO 6383-2
Dart Drop Test 120 gASTM 1709A, ISO 7765
Film Tensile Strength at Break, MD 57.0 MPaASTM D882
Film Tensile Strength at Break, TD 38.0 MPaASTM D882
1% Secant Modulus, MD 220 MPaASTM D882
1% Secant Modulus, TD 250 MPaASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 120 °CASTM D3418, ISO 3146
 
Optical PropertiesOriginal ValueComments
Haze 9.0 %ASTM D1003
Gloss 47 %@ 45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PETHYD910 / 200056

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.