MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Alclad Aluminum 7178-T6, T651
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition for AA 7178 (not Alclad 7178 specifically).
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A87178; Alclad 7178-T6, T651; Alclad 7178-T6, T651; Al7178-T6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.83 g/cc0.102 lb/in³For AA7178 (Not Alclad)
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 558 MPa81000 psiAA; Typical
Tensile Strength, Yield 490 MPa71000 psiAA; Typical
Elongation at Break 10 %
@Thickness 1.59 mm
10 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 71.7 GPa10400 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Shear Strength 330 MPa47900 psiCalculated
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 468 °C875 °F
Aging Temperature 121 °C250 °Ffor 24 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 85.3 - 89.5 %85.3 - 89.5 %As remainder
Chromium, Cr 0.18 - 0.28 %0.18 - 0.28 %
Copper, Cu 1.6 - 2.4 %1.6 - 2.4 %
Iron, Fe <= 0.50 %<= 0.50 %
Magnesium, Mg 2.4 - 3.1 %2.4 - 3.1 %
Manganese, Mn <= 0.30 %<= 0.30 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.40 %<= 0.40 %
Titanium, Ti <= 0.20 %<= 0.20 %
Zinc, Zn 6.3 - 7.3 %6.3 - 7.3 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 7178-T6; 7178-T651
Alclad Aluminum 7075-T6, T651
Aluminum 7001-T6; 7001-T651
Aluminum 7075-T6; 7075-T651
Aluminum 7175-T66

MA7178AT6 / 9618

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.