MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Wacker Elastosil® R plus 4370/50 Silicone Rubber
Categories: Polymer; Thermoset; Silicone; Silicone Rubber

Material Notes: ELASTOSIL® R plus 4370/50 is a self-adhesive addition-curing compound for the manufacture of extruded, coated or molded articles.

Properties: ELASTOSIL® R plus 4370/50 adheres to steel, aluminum, thermoplastics (e.g. PBT) with good heat deflection temperature, to synthetic fibers (such as polyester), as well as to other silicones without any primering or special surface treatments.

Application: ELASTOSIL® R plus 4370/50 is intended for the manufacture of 2-composite combinations via pressure free extrusion or co-extrusion. ELASTOSIL® R plus 4370/50 can generally be used for technical applications without post-curing.

Information provided by Wacker Chemie AG.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³DIN 53479
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 4848DIN 53505
Tensile Strength at Break 9.90 MPa1440 psiDIN 53504 S1
Elongation at Break 900 %900 %DIN 53504 S1
Rebound 55 %55 %DIN 53512
Tear Strength 42.0 kN/m240 pliASTM D624 B
 
Processing PropertiesMetricEnglishComments
Cure Time 15.0 min
@Treatment Temp. 165 °C
0.250 hour
@Treatment Temp. 329 °F
 
Descriptive Properties
Appearancetranslucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PWACK9298 / 204827

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.