MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Celanese Celanex® 6500LM PBT, 30% Mineral / Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass + Mineral Filled

Material Notes: Celanex 6500 is a 30% glass/mineral polyester with improved surface finish and a good balance of mechanical properties and processability, that is also enhanced for improved laser marking graphics.
To avoid hydrolytic degradation during processing, CELANEX resins have to be dried to a moisture level equal to or less than 0.02%. Drying should be done in a dehumidifying hopper dryer capable of dewpoints <-40°F (-40°C) at 250°F (121°C) for 4 hours.
For subsequent storage of the material in the dryer until processed (<= 60 h) it is necessary to lower the temperature to 100° C.

Information provided by Celanese Corporation.

Key Words: 30% glass/mineral, low warp, laser markable
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.55 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0020 - 0.0050 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 125 MPa5mm/min; ISO 527-2/1A
 18000 psi
@Temperature 22.8 °C
ASTM D638
Elongation at Break 2.2 %5mm/min; ISO 527-2/1A
 3.0 %
@Temperature 22.8 °C
ASTM D638
Tensile Modulus 9700 MPa1mm/min; ISO 527-2/1A
Flexural Strength 180 MPaISO 178
 28000 psi
@Temperature 22.8 °C
ASTM D790
Flexural Modulus 9500 MPaISO 178
 1.35e+6 psi
@Temperature 22.8 °C
ASTM D790
Izod Impact, Notched 1.40 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Izod Impact, Notched (ISO) 5.30 kJ/m²ISO 180/1A
Charpy Impact Unnotched 30.0 kJ/m²ISO 179/1eU
 30.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 7.10 kJ/m²ISO 179/1eA
 6.40 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 28.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 85.0 µm/m-°CISO 11359-2
Melting Point 225 °CISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 223 °CISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 202 °CISO 75-1, -2
Flammability, UL94 HB
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 50.0 °Chopper
 65.0 - 96.0 °Ccavity
Feed Temperature 230 - 250 °C
Zone 1 230 - 250 °C
Zone 2 235 - 255 °C
Zone 3 235 - 255 °C
Zone 4 240 - 265 °C
Die Temperature 240 - 265 °C
Melt Temperature 235 - 265 °C
 260 °CISO 294
Mold Temperature 82.0 °CISO 294
Injection Velocity 300 mm/secISO 294
Drying Temperature 120 - 130 °C
Dry Time 4 hour
Moisture Content 0.020 %Necessary low maximum
Injection Pressure 48.0 MPaISO 294
Hot-Working Temperature 250 - 265 °C
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultradur® B 4300 G6 30% Glass Filled PBT
Evonik Vestodur® GF30 30% Glass Reinforced Laser Markable PBT
SAES Getters Nd:YAG Solid State Laser Crystals (Nd-doped Y3Al5O12)
Celanese Celanex® 1462Z PBT, 30% Glass Reinforced
Celanese Celanex® 2300 GV1/30 PBT, 30% Glass Reinforced

PHCS094 / 123509

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.