MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

CRP Technology Windform® LX 3.0 Polyamide-Glass Fiber Composite for SLS
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Processed by selective laser sintering (SLS). Windform® LX 3.0 maintains the Windform® LX 2.0’s technical and thermal properties; it is also not electrically conductive. It is a naturally black material and is characterized by good Tensile Strength and stiffness. Windform® LX 3.0 is also characterized by high level of temperature resistance (HDT, 1.82 Mpa is 175,9°C / 348.62 °F). It has an excellent surface finish in its sintered state; it is perfect for components with fine details. Windform® LX 3.0 is highly recommended for applications that require a strong visual impact and for aesthetical parts. Its impact resistance properties at room and low temperature are similar. Windform® LX 3.0 is an entry-level material and is perfect for creating functional prototypes or finished parts that require reliability, resistance and aesthetical properties.

Applications Windform® LX 3.0 is perfect for complex parts, as well as assembly testing. It is a suitable material to create fully functional applications which do not require high resistance to mechanical stress. There are several fields of application: covers, latching systems, air intake systems, connectors, driver cockpit components. Cooling/ducted fans, UAV structural components, design parts. It is the material of choice for electrically insulated prototypes. Windform® LX 3.0 is perfect for creating battery boxes, containers of electrical and electronic components.

Information provided by CRP Technology.

Vendors:   About CRP Technology
CRP Technology (Modena, Italy) develops, manufactures and sells its proprietary high performance composite materials Windform® for professional 3D Printing. It is also distinguished by its know-how in Selective Laser Sintering technology. It offers part production for short- and low-run production, and prototyping services with Windform®. Its specific application fields including but are not limited to: automotive and motorsports, design, aerospace, UAVs, marine, entertainment, defense, and packaging.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.324 g/cc0.04783 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 60.42 MPa8763 psiUNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Elongation at Break 2.42 %2.42 %UNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Tensile Modulus 6.048 GPa877.2 ksiUNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Flexural Strength 85.80 MPa12440 psiUNI EN ISO 14125: 2000
Flexural Modulus 5.465 GPa792.6 ksiUNI EN ISO 14125: 2000
Charpy Impact Unnotched 1.882 J/cm²8.957 ft-lb/in²Completely broken specimens; UNI EN ISO 179
Charpy Impact, Notched  0.483 J/cm²
@Temperature -40.0 °C
2.30 ft-lb/in²
@Temperature -40.0 °F
UNI EN ISO 179-1
 0.533 J/cm²
@Temperature 23.0 °C
2.54 ft-lb/in²
@Temperature 73.4 °F
UNI EN ISO 179-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.7e+13 ohm-cm1.7e+13 ohm-cmASTM D257-93
Surface Resistance 6.8e+15 ohm6.8e+15 ohmASTM D257-93
Comparative Tracking Index 600 V600 VIEC 60112:2003
 
Thermal PropertiesMetricEnglishComments
Melting Point 183.3 °C361.9 °FISO 11357-2
Deflection Temperature at 1.8 MPa (264 psi) 175.9 °C348.6 °FASTM D 648 TYPE B
Vicat Softening Point 178.8 °C353.8 °F10 N; ASTM D1525-09
 
Descriptive Properties
ColorBlack
Specific Flexural Modulus4128[MPa/(g/cc)], Flexural Modulus per density unit
Specific Flexural Strength64.8[MPa/(g/cc)], Flexural Strength per density unit
Specific Tensile Modulus4568[MPa/(g/cc)], Tensile Modulus per density unit
Specific Tensile Strength45.6[MPa/(g/cc)], UTS per density unit
Surface Finish1.2 Ra µmAfter CNC machining
 3.2 Ra µmAfter Manual Finishing
 7.5 Ra µmAfter SLS Process

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ALM FR 106 Nylon 11 SLS Prototyping Polymer
ALM PA 615-GF Nylon 12 SLS Prototyping Polymer, 50% Glass Filled
3D Systems DuraForm® EX Impact-Resistant Plastic for SLS® Systems
3D Systems DuraForm® HST Fiber Filled Nylon for SLS Systems
ALM PA 650 Nylon 12 SLS Prototyping Polymer

PCRPT40c / 209869

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.