MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Eastman Provista UVI Copolymer
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Provista UVI is a Provista copolymer with an indoor/outdoor UV package added to prevent yellowing caused by light. Provista copolymer is a resin specifically developed for extrusion into profiles where aesthetics like high clarity and gloss, coupled with design flexibility drive demand. Compared to commonly used materials, Provista copolymer can often run on most standard processing equipment at increased speeds. An extremely high melt strength makes the resin an excellent choice when extruding profiles into complicated shapes. This product is certified to ANSI/NSF Standard 51.

Applications/Uses

  • Candy Packaging
  • Pricing channels
  • Tubing
  • Point of purchase displays
  • Food packaging
  • Furniture guards
  • Teething rails
  • Key Attributes

  • Ease of processing
  • Excellent chemical resistance
  • Sparkling clarity and high gloss
  • Toughness with flexibility
  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Specific Gravity 1.27 g/ccASTM D792
     
    Mechanical PropertiesOriginal ValueComments
    Hardness, Rockwell R 106ASTM D785
    Tensile Strength at Break 29.0 MPaASTM D638
    Tensile Strength, Yield 50.0 MPaASTM D638
    Elongation at Break 109 %ASTM D638
    Elongation at Yield 4.0 %ASTM D638
    Flexural Strength 72.0 MPaASTM D790
    Flexural Modulus 2.20 GPaASTM D790
    Izod Impact, Notched 0.520 J/cm
    @Temperature -40.0 °C
    ASTM D256
     94.0 J/m
    @Temperature 23.0 °C
    ASTM D256
    Izod Impact, Unnotched NBASTM D4812
     NB
    @Temperature -40.0 °C
    ASTM D4812
    Puncture Energy 33.0 JPuncture Resistance @Max Load, 23°C; ASTM D3763
     37.0 JPuncture Resistance @Max Load, 0°C; ASTM D3763
     41.0 J
    @Temperature -40.0 °C
    Puncture Resistance at Max Load; ASTM D3763
     
    Thermal PropertiesOriginal ValueComments
    Deflection Temperature at 0.46 MPa (66 psi) 67.0 °CASTM D648
    Deflection Temperature at 1.8 MPa (264 psi) 62.0 °CASTM D648
    Vicat Softening Point 79.0 °C1kg load; ASTM D1525
     
    Optical PropertiesOriginal ValueComments
    Haze 0.60 %ASTM D1003
    Gloss 171 %at 60°; ASTM D2457
    Transmission, Visible 89 %Regular Transmittance; ASTM D1003
     90 %Total Transmittance; ASTM D1003
     
    Descriptive Properties
    Color, CIE b*0.61

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Dow Pellethane® 2354-45D Polyurethane Elastomer, Polyester Polycaprolactone Based
    Dow Pellethane® 2102-90AE Polyurethane Elastomer, Polyester Polycaprolactone Based
    Dow Pellethane® 2102-85A Polyurethane Elastomer, Polyester Polycaprolactone Based
    Covestro Makroblend® UT-403 Polycarbonate + Polyester Blend
    C.O.I.M. LARIPUR® LPR8020 Standard Adipate Ester Polyurethane

    PE9095 / 35151

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.