MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Chesterton ARC I BX1 RC Ceramic-Filled Epoxy/Urethane Industrial Coating
Categories: Polymer; Thermoset; Epoxy; Polyurethane, TS

Material Notes: A rapid curing high impact resistant, 100% solids, epoxy/urethane hybrid with ceramic reinforcements for severe wear regions & impact. ARC I BX1 RC industrial coating is designed to: Cure quickly allowing a faster turn-around with repairs; Coat & protect surfaces exposed to moderate to severe impact & sliding abrasion; Rapidly repair/replace cracked ceramic tile or rubber lining where impact forces combined with sliding wear tear seams and edges; Resist direct and reverse impact forces associated with materials handling system; Easily apply by trowel

Filler: Blend of sintered bauxite beads & SiC powders treated with polymeric coupling agent. Matrix: A modified epoxy/urethane resin hybrid reacted with a fast curing amine curing agent.

Information provided by Chesterton

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.36 g/cc0.0853 lb/in³Cured
Solids Content 100 %100 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8383ASTM D2240
Tensile Strength at Break 19.7 MPa2850 psiASTM D638
Elongation at Break 1.7 %1.7 %ASTM D638
Flexural Strength 41.4 MPa6000 psiASTM D790
Flexural Modulus 4.96 GPa720 ksiASTM C580
Compressive Strength 66.2 MPa9600 psiASTM D695
Adhesive Bond Strength 23.4 MPa3390 psiPull-Off Adhesion; ASTM D4541
Impact Test >= 20.3 J>= 15.0 ft-lbReverse Impact; ASTM D2794
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 95.0 °C203 °FWet Service
 205 °C401 °FDry Service
 
Processing PropertiesMetricEnglishComments
Shelf Life 24.0 Month
@Temperature 10.0 - 32.0 °C
24.0 Month
@Temperature 50.0 - 89.6 °F
Dry, Unopened Containers
 
Descriptive Properties
ColorBrown
Vertical Sag Resistance,No Sag21°C (70°F) and 375 µm (15 mil)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPTCHS025c / 239856

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.