MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
CLAL-MSX NICLAFOR® 1000 TD4 Quenched/Cold Rolled, Drawn Copper Alloy
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Finished parts can be produced with: reduction in sections, high mechanical properties even at high temperature, high spring properties, high conductivity, good resistance to corrosion, low permeability, good formability, long life duration. Meets environmental concern by not containing Beryllium, Cadmium nor Titanium.

Applications:

  • Electrotechnic
  • Electromechanic
  • Electronic
  • Connectic
  • Automotive
  • Domestic appliances
  • Spectacle industry
  • Turned parts.

Information provided by CLAL-MSX

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.90 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 230 - 300
Tensile Strength, Ultimate 780 - 880 MPa
Tensile Strength, Yield >= 700 MPa
@Strain 0.2 %
Elongation at Break >= 1.5 %A50 mm
Modulus of Elasticity 120 GPa
Modulus of Rigidity 50.0 GPaTorsion
Fatigue Strength 450 MPa
@# of Cycles 1.00e+7
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity <= 0.00001433 ohm-cmprecipitation hardened (3h)
 <= 0.00001911 ohm-cmquenched
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.25 µm/m-°C
@Temperature 20.0 - 200 °C
Thermal Conductivity 53.6 W/m-K
Melting Point 968 - 1078 °C
Solidus 968 °C
Liquidus 1078 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 82.65 - 85.95 %
Iron, Fe <= 0.50 %
Lead, Pb <= 0.030 %
Manganese, Mn 0.050 - 0.30 %
Nickel, Ni 8.5 - 9.5 %
Phosphorus, P <= 0.020 %
Tin, Sn 5.5 - 6.5 %
Zinc, Zn <= 0.50 %
 
Descriptive Properties
Striction>60%Coef. Z

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals INCONEL® 706 Precipitation Hardening Alloy, Cold Rolled Sheet, Solution Treated
ArcelorMittal MartINsite® 1200 Cold Rolled Steel
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, 30% Cold Rolled (UNS S30400)
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, 60% Cold Rolled (UNS S30400)
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, 60% Cold Rolled (UNS S30403)

NCLAL072 / 160103

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.