MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
NOVA Chemicals Novapol® TF-0338-E Hexene LMDPE Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Medium Density (MDPE); Linear Medium Density Polyethylene (LMDPE), Film

Material Notes: Excellent stiffness and gloss

Applications: Diaper back sheet, Blending

Additives: High temperature AO

Film properties are typical of film extruded at 280°C.

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.938 g/ccASTM D792
Melt Flow 3.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 15.0 MPaASTM D882
Film Tensile Strength at Yield, TD 16.0 MPaASTM D882
Film Elongation at Break, MD 800 %ASTM D882
Film Elongation at Break, TD 1070 %ASTM D882
Secant Modulus, MD 0.320 GPaat 1%; ASTM D882
Secant Modulus, TD 0.380 GPaat 1%; ASTM D882
Impact 80J/mm; NOVA Chemicals Puncture test
Coefficient of Friction >= 0.80ASTM D1894
Elmendorf Tear Strength, MD 1.40 g/micronASTM D1922
Elmendorf Tear Strength, TD 8.00 g/micronASTM D1922
Film Tensile Strength at Break, MD 41.0 MPaASTM D882
Film Tensile Strength at Break, TD 32.0 MPaASTM D882
 
Optical PropertiesOriginal ValueComments
Haze 4.0 %ASTM D1003
Gloss 87 %at 45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Petromont 2100 Medium Density Polyethylene Resin
NOVA Chemicals Sclair® 2514 MDPE Injection Molding Resin
NOVA Chemicals Sclair® 2515 MDPE Injection Molding Resin
LyondellBasell Lupolen 3821 D MDPE
Chevron Phillips mPact™ D353 m-MDPE Linear Low Density Polyethylene

PNOVA150 / 55051

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.