MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Alcoloy Copper, UNS C68800, H01 Temper strip
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold formability. Fabricated by blanking, drawing, forming and bending, shearing and stamping.

Applications: springs, switches, contacts, relays, drawn parts.

Test specimen: strip - 1mm thickness.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.20 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 90.590.5
Hardness, Rockwell 30T 7878
Tensile Strength, Ultimate 650 MPa94300 psi
Tensile Strength, Yield 525 MPa
@Strain 0.2 %
76100 psi
@Strain 0.2 %
Elongation at Break 20 %20 %In 50 mm
Modulus of Elasticity 116 GPa16800 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000210 ohm-cm0.0000210 ohm-cm8.2% IACS
Magnetic Permeability 1.0031.003
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 µm/m-°C
@Temperature 20.0 - 300 °C
10.0 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.375 J/g-°C0.0896 BTU/lb-°F
Thermal Conductivity 69.0 W/m-K479 BTU-in/hr-ft²-°F
Melting Point 950 - 965 °C1740 - 1770 °F
Solidus 950 °C1740 °F
Liquidus 965 °C1770 °F
Annealing Point 399 - 593 °C750 - 1100 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.0 - 3.8 %3.0 - 3.8 %
Cobalt, Co 0.25 - 0.55 %0.25 - 0.55 %
Copper, Cu 72.3 - 74.7 %72.3 - 74.7 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.050 %<= 0.050 %
Other, total <= 0.010 %<= 0.010 %
Zinc, Zn 22.7 %22.7 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chromium-Bearing Copper-Nickel, UNS C71900, Heat Treated
Cartridge Brass, UNS C26000 (260 Brass), OS035 Temper wire
Arsenical Naval brass, UNS C46500, H01 Temper 1 mm flat products
Antimonial Admiralty Copper, UNS C44400, H01 Temper tubing
Ampco Metal AMPCO® 483 Aluminum-Nickel Bronze, Extruded Rod, 50.8 - 76.2 mm.

MC68800b4 / 11686

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.