MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Wellman Wellamid® FRGF25-66-N Flame Retardant Nylon 66, Lubricated, 25% Glass Fiber  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass Fiber Filled, Flame Retardant

Material Notes: Typical Applications: Electrical terminal blocks, electric fan switch housings, coil forms, multi-pin electrical connectors, electric fan switch housings, TV tuner components, automotive switch housings.

Data provided by the manufacturer, Wellman Inc.

Key Words: Polyamide 66
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.40 g/cc0.0506 lb/in³ISO 1183
Water Absorption 1.4 %1.4 %Approximate 24 hr.
Linear Mold Shrinkage 0.0030 - 0.0070 cm/cm0.0030 - 0.0070 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 110 MPa16000 psiISO 527
Elongation at Break 2.0 %2.0 %ISO 527
Flexural Yield Strength 165 MPa23900 psiISO 178
Flexural Modulus 6.70 GPa972 ksiISO 178
Izod Impact, Notched 0.400 J/cm0.749 ft-lb/inISO 180
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 240 °C464 °FISO 75
Flammability, UL94 V-0
@Thickness 0.790 mm
V-0
@Thickness 0.0311 in
UL 94
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 271 - 282 °C520 - 540 °F
Middle Barrel Temperature 266 - 277 °C510 - 530 °F
Front Barrel Temperature 260 - 271 °C500 - 520 °F
Nozzle Temperature 271 - 282 °C520 - 540 °F
Melt Temperature 266 - 277 °C510 - 530 °F
Mold Temperature 71.1 - 93.3 °C160 - 200 °F
Drying Temperature 79.4 °C175 °FOpened bags and gaylord boxes
Dry Time 2 - 4 hour2 - 4 hourOpened bags and gaylord boxes
Moisture Content 0.050 - 0.20 %0.050 - 0.20 %During molding to prevent hydrolytic degradation
 <= 0.20 %<= 0.20 %In shipping bags, ready to mold
Injection Pressure 34.5 - 138 MPa5000 - 20000 psi
Back Pressure 0.345 MPa50.0 psi
Screw Speed 30 - 120 rpm30 - 120 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
SPS Guang Zhou PONYL™ EP4003G25 Non-halogen flame retardance/GF25%-PA66
RTP Company RTP 204 FR XB Nylon 6/6 (PA) Glass Fiber - Flame Retardant - Black Color Only
RTP Company RTP 204 FR HS  Nylon 6/6 (PA 6/6) Glass Fiber 25% - Flame Retardant - Heat Stable
LATI Latiohm 66-04 PD01 G/25-V0CT1 PA66, 25% Glass Fiber Reinforced, Flame Retardant
LATI Latamid 66 H2 G/25-V0CT1 PA 66, 25% Glass Fiber Reinforced, Heat Stabilized, Flame Retardant

PWEL52 / 72332

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.