MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Prodways PLASTCure Alumina Powder for 3D Printing
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: PLASTCure Alumina is a ceramic resin which was developed for manufacturing high-quality prototypes or end-use parts in several industries, including parts like supports for heating elements, grinding parts, mechanical components, high-temperature electric insulators and insulating rings.

Information provided by Prodways

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Porosity 0.70 %Finished Product
Viscosity 13000 cPPaste
 
Mechanical PropertiesOriginal ValueComments
Vickers Microhardness 2.1GPa
Modulus of Elasticity 0.380 GPa
Flexural Strength 1100 MPa
Compressive Strength 3500 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+15 ohm-cm
Dielectric Strength 18.0 kV/mm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.50 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.900 J/g-°C
@Temperature 20.0 °C
Thermal Conductivity 25.0 W/m-K
@Temperature 100 °C
Maximum Service Temperature, Air 1700 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik Osprey 1.2709 Tool Steel Powder
Prodways PLASTCure Model 310 Liquid Resin for 3D Printing
Prodways PLASTCure ABS 3650 3D Printing Polymer
Lubriplate 1444 Aluminum Complex Multi-Purpose Grease
EOS PH1 Precipitation Hardening Stainless Steel Sintered on EOSINT M 270

PPRODW963 / 220981

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.