MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Epsan Eplamid 66 IMP NC Q1B802 Polyamide 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Unreinforced and modified polyamide 66, with improved good-impact resistance, heat stabilized, lubricated for injection molding. Eplamid 66 IMP offers an excellent notched high impact resistance and ensures outstanding performance at low temperatures, making it suitable for all sectors of industries and for applications such as sports & leisure and automotive industries.

Information provided by Epsan Plastik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.08 g/cc0.0390 lb/in³ISO 1183
Linear Mold Shrinkage 0.018 cm/cm0.018 in/inParallel; ISO 294-4
 0.022 cm/cm0.022 in/inNormal; ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Stress 35.0 MPa5080 psiConditioned; ISO 527-2
 50.0 MPa7250 psiDry; ISO 527-2
Elongation at Break >= 50 %>= 50 %Dry; ISO 527-2
 >= 50 %>= 50 %Conditioned; ISO 527-2
Tensile Modulus 1.10 GPa160 ksiConditioned; ISO 527-2
 2.05 GPa297 ksiDry; ISO 527-2
Flexural Strength 70.0 MPa10200 psiISO 178
Flexural Modulus 1.85 GPa268 ksiISO 178
Izod Impact, Notched (ISO) 70.0 kJ/m²33.3 ft-lb/in²ISO 180/1A
Charpy Impact, Notched 7.50 J/cm²35.7 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 260 °C500 °FISO 3146
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
EN 60695-11-10
 
Processing PropertiesMetricEnglishComments
Processing Temperature 280 °C536 °FRecommended Injection Molding Temperature
Drying Temperature 80.0 °C176 °FAverage Drying Time is 2-4 hrs
Moisture Content 0.20 %0.20 %ISO 15512

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEPSAN084 / 186398

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.