MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Plenco 4527 Phenolic, Granular, Injection Molded
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic; Phenolic, Resole, Mineral/Flock Filled

Material Notes: PLENCO 04527 is a heat resistant, mineral and flock filled phenolic molding compound, offering excellent mechanical strength, and resistance to cracking in a wet-dry environment. UL recognized under component file E40654. 04527 is available in black.

Information supplied by Plenco.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.620 g/cc0.0224 lb/in³ASTM D1895
Density 1.58 g/cc0.0571 lb/in³ASTM D792
Water Absorption 0.40 %0.40 %ASTM D570
Linear Mold Shrinkage 0.0053 cm/cm0.0053 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 5757ASTM D785
Tensile Strength, Ultimate 53.0 MPa7690 psiASTM D638
Elongation at Break 0.85 %0.85 %ASTM D638
Tensile Modulus 10.1 GPa1460 ksiASTM D638
Flexural Strength 79.0 MPa11500 psiASTM D790
Flexural Modulus 8.60 GPa1250 ksiASTM D790
Compressive Strength 139 MPa20200 psiASTM D695
Poissons Ratio 0.340.34ASTM D638
Shear Modulus 3.77 GPa547 ksiCalculated
Izod Impact, Notched 0.190 J/cm0.356 ft-lb/inASTM D256
Charpy Impact, Notched 0.205 J/cm²0.976 ft-lb/in²ASTM D256
Impact 144144J/m Drop Ball Impact; PLENCO
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.70e+12 ohm-cm1.70e+12 ohm-cmASTM D247
Dielectric Constant 6.56.5ASTM D150
Dielectric Strength 7.30 kV/mm185 kV/inStep by Step; ASTM D149
 9.40 kV/mm239 kV/inShort Time; ASTM D149
Dissipation Factor 0.1620.162ASTM D150
Arc Resistance 181 sec181 secASTM D495
Comparative Tracking Index 200 V200 VASTM D3638
 
Thermal PropertiesMetricEnglishComments
CTE, linear 34.0 µm/m-°C
@Temperature 40.0 - 130 °C
18.9 µin/in-°F
@Temperature 104 - 266 °F
TMA; ASTM E831
Thermal Conductivity 0.550 W/m-K
@Temperature 100 °C
3.82 BTU-in/hr-ft²-°F
@Temperature 212 °F
ASTM E1461
Maximum Service Temperature, Air 202 °C396 °FHeat Resistance; ASTM D570D
Deflection Temperature at 1.8 MPa (264 psi) 204 °C399 °FASTM D648
Flammability, UL94 V-1
@Thickness 1.50 mm
V-1
@Thickness 0.0591 in
Oxygen Index 31 %31 %ASTM D2863
Shrinkage 0.34 %0.34 %72 hr, 120ºC; ASTM D1299

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Plenco 2369 Phenolic, Granular, Compression Molded
Plenco 2311 Phenolic, Granular, Transfer Molded
Plenco 2311 Phenolic, Granular, Injection Molded
Plenco 2308 Phenolic, Granular, Transfer Molded
Plenco 2308 Phenolic, Granular, Injection Molded

PLEL91 / 50666

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.