MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Pressure Seal 55788 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 55788 is a 70 durometer black colored highly saturated nitrile ( HSN ) elastomer, it is specifically formulated to be electrically conductive. It exhibits good resistance to abrasion and petroleum based oils.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 725 EO14 EO34 F19; 3 BG 730 B14 F19; 4 BG 730 A14 B14 F19; 2 BG 725 EA14 EF11 EF21 EO14 EO34 F17; 5 BG 720 A14 EO14 EO34 F17; 2 CH 725 A25 EO35 F17; 3 CH 725 A25 EO16 EO36; 5 CH 720 A25 B14 F14; 6 CH 720 A15 EO36 F17

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.10 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 75
 56
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 61
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 70
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
 71
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 71
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 71
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 75
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 75
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 78
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 79
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 80
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 84
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 85
@Temperature 150 °C,
Time 252000 sec
Heat Aged
Tensile Strength 3968 psi
 1372.9 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 2182.4 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 3864.8 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 3987.8 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
 4031.5 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 4182.3 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 4182.3 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 4456.1 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 4464 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 4523.5 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 4551.3 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 4833 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 529 %
 241.8 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 349.1 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 415.8 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 502.1 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 512.07 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 512.07 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 523.2 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 525.8 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 529 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 537.993 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 543.3 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 544.9 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
100% Modulus 490 psi
Tear Strength 310 pliDie C
 367 pliDie B
Compression Set 28.2 %
@Temperature 100 °C,
Time 79200 sec
Solid
 33.6 %
@Temperature 100 °C,
Time 252000 sec
Solid
 40.4 %
@Temperature 100 °C,
Time 79200 sec
Plied
 44.7 %
@Temperature 100 °C,
Time 252000 sec
Plied
 59.5 %
@Temperature 150 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -72.0 °F
Shrinkage -5.50 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -5.20 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -0.300 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 0.60 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 10.9 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 12.2 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #3
 14.3 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 14.3 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 31.4 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 55 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL052 / 318262

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.