System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
660 Stainless Steel (A286) short time tensile test
Categories:
Metal
;
Ferrous Metal
;
Heat Resisting
;
Stainless Steel
;
T 600 Series Stainless Steel
Key Words:
UNS S66286 (UNS K66286), AMS 5525, AMS 5731, AMS 5732, AMS 5734, AMS 5735, AMS 5736, AMS 5737, AMS 5804, AMS 5805, ASME SA638, ASTM A453, ASTM A638, SAE J467 (A286); DIN 1.4980
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
7.92
g/cc
Mechanical Properties
Original Value
Comments
Tensile Strength, Ultimate
1007
MPa
Tensile Strength, Yield
703
MPa
@Strain 0.2 %
569 at 0.02% offset
213
MPa
@Strain 0.2 %,
Temperature 815 °C
307
MPa
@Strain 0.2 %,
Temperature 760 °C
472
MPa
@Strain 0.2 %,
Temperature 705 °C
603
MPa
@Strain 0.2 %,
Temperature 540 °C
427 at 0.02% offset
607
MPa
@Strain 0.2 %,
Temperature 650 °C
431 at 0.02% offset
621
MPa
@Strain 0.2 %,
Temperature 595 °C
445 at 0.02% offset
645
MPa
@Strain 0.2 %,
Temperature 370 °C
490 at 0.02% offset
645
MPa
@Strain 0.2 %,
Temperature 425 °C
496 at 0.02% offset
645
MPa
@Strain 0.2 %,
Temperature 205 °C
524 at 0.02% offset
810
MPa
@Strain 0.2 %,
Temperature -75.0 °C
889
MPa
@Strain 0.2 %,
Temperature -195 °C
Elongation at Break
25 %
in 50 mm
11 %
@Temperature 705 °C
in 50 mm
13 %
@Temperature 650 °C
in 50 mm
18.5 %
@Temperature 760 °C
in 50 mm
18.5 %
@Temperature 425 °C
in 50 mm
18.5 %
@Temperature 540 °C
in 50 mm
21 %
@Temperature 595 °C
in 50 mm
21.5 %
@Temperature 205 °C
in 50 mm
22 %
@Temperature 370 °C
in 50 mm
30 %
@Temperature -75.0 °C
in 50 mm
35 %
@Temperature -195 °C
in 50 mm
68.5 %
@Temperature 815 °C
in 50 mm
Reduction of Area
36.8 %
9.6 %
@Temperature 705 °C
14.5 %
@Temperature 650 °C
23 %
@Temperature 595 °C
23.4 %
@Temperature 760 °C
31.2 %
@Temperature 540 °C
35 %
@Temperature 425 °C
37.5 %
@Temperature 815 °C
45 %
@Temperature 370 °C
52.8 %
@Temperature 205 °C
Modulus of Elasticity
200
GPa
Typical for stainless steel
Charpy Impact
87.0
J
@Diameter 22.0 mm
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
48.0
J
@Diameter 22.0 mm,
Temperature 650 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
60.0
J
@Diameter 22.0 mm,
Temperature 705 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
60.0
J
@Diameter 22.0 mm,
Temperature 595 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
62.0
J
@Diameter 22.0 mm,
Temperature 540 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
70.0
J
@Diameter 22.0 mm,
Temperature 425 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
75.0
J
@Diameter 22.0 mm,
Temperature 760 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
75.0
J
@Diameter 22.0 mm,
Temperature 370 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
77.3
J
@Diameter 22.0 mm,
Temperature -195 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
81.0
J
@Diameter 22.0 mm,
Temperature 205 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
92.2
J
@Diameter 22.0 mm,
Temperature -75.0 °C
V-Notch; Conditions prior to test: bar ST980°C; OQ; Aged 16 hr at 720°C, AC.
Thermal Properties
Original Value
Comments
CTE, linear
16.9
µm/m-°C
@Temperature 21.0 - 100 °C
solution treated, 16.7 solution treated and aged.
17.2
µm/m-°C
@Temperature 20.0 - 250 °C
17.4
µm/m-°C
@Temperature 21.0 - 500 °C
17.6
µm/m-°C
@Temperature 21.0 - 650 °C
solution treated
17.7
µm/m-°C
@Temperature 21.0 - 750 °C
solution treated
18.5
µm/m-°C
@Temperature 21.0 - 750 °C
solution treated and aged.
19.4
µm/m-°C
@Temperature 21.0 - 900 °C
solution treated
Specific Heat Capacity
0.460
J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity
12.6
W/m-K
@Temperature 21.0 °C
15.1
W/m-K
@Temperature 150 °C
20.2
W/m-K
@Temperature 425 °C
23.79
W/m-K
@Temperature 600 °C
24.7
W/m-K
@Temperature 650 °C
Melting Point
1370
-
1425
°C
Solidus
1370
°C
Liquidus
1425
°C
Maximum Service Temperature, Air
815
°C
Continuous Service
980
°C
Intermittent
Component Elements Properties
Original Value
Comments
Aluminum, Al
<= 0.035 %
Boron, B
0.0010 - 0.010 %
Carbon, C
<= 0.080 %
Chromium, Cr
13.5 - 16 %
Copper, Cu
<= 0.25 %
Iron, Fe
56 %
Manganese, Mn
<= 2.0 %
Nickel, Ni
24 - 27 %
Phosphorus, P
<= 0.040 %
Silicon, Si
<= 1.0 %
Sulfur, S
<= 0.030 %
Titanium, Ti
1.9 - 2.35 %
Vanadium, V
0.10 - 0.50 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
316 Stainless Steel, annealed bar
304 Stainless Steel (UNS S30400); Annealed Bar
303 Stainless Steel, annealed bar
Titanium Ti-6Al-4V (Grade 5), Annealed
Crucible Steel 431 Chromium Steel
MQ660AC / 13246
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.