MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ExxonMobil AP03B Polypropylene Impact Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Impact Modified; Molded/Extruded

Material Notes: Product Description: A high crystallinity, medium impact copolymer resin with high melt flow rate and excellent processing attributes. It is designed for injection molded large appliance applications and automotive interior parts.

Availability: Asia Pacific

Features:

  • Fast Molding Cycle
  • Good Processability
  • High Flow
  • High Stiffness
  • Highly Crystalline
  • Medium Impact Resistance
Uses:
  • Appliance Components
  • Automotive Applications
  • Automotive Interior Parts
  • Consumer Applications
  • Industrial Applications

Processing Method: Injection Molding

Information provided by ExxonMobil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ExxonMobil Method
Melt Flow 30 g/10 min
@Load 2.16 kg,
Temperature 230 °C
30 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 25.1 MPa3640 psiISO 527-2/50
 26.6 MPa3860 psi2.0 in/min; ASTM D638
Elongation at Yield 4.9 %4.9 %ISO 527-2/50
 5.0 %5.0 %2.0 in/min; ASTM D638
Tensile Modulus 1.44 GPa209 ksiISO527-2/1
Flexural Modulus 1.26 GPa183 ksi0.079 in/min; ISO 178
Flexural Modulus, 1% Secant 1310 MPa190000 psi0.05 in/min; ASTM D790A
 1500 MPa217000 psi0.5 in/min; ASTM D790B
Izod Impact, Notched  0.342 J/cm
@Temperature -17.8 °C
0.640 ft-lb/in
@Temperature 0.000 °F
ASTM D256A
 0.694 J/cm
@Temperature 22.8 °C
1.30 ft-lb/in
@Temperature 73.0 °F
ASTM D256A
Izod Impact, Notched (ISO)  2.94 kJ/m²
@Temperature -40.0 °C
1.40 ft-lb/in²
@Temperature -40.0 °F
ISO 180/1A
 3.99 kJ/m²
@Temperature -17.8 °C
1.90 ft-lb/in²
@Temperature 0.000 °F
ISO 180/1A
 7.98 kJ/m²
@Temperature 22.8 °C
3.80 ft-lb/in²
@Temperature 73.0 °F
ISO 180/1A
Charpy Impact, Notched  0.336 J/cm²
@Temperature -30.0 °C
1.60 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.378 J/cm²
@Temperature -20.0 °C
1.80 ft-lb/in²
@Temperature -4.00 °F
ISO 179/1eA
 0.420 J/cm²
@Temperature 0.000 °C
2.00 ft-lb/in²
@Temperature 32.0 °F
ISO 179/1eA
 0.756 J/cm²
@Temperature 22.8 °C
3.60 ft-lb/in²
@Temperature 73.0 °F
ISO 179/1eA
Gardner Impact 17.3 J
@Thickness 3.17 mm,
Temperature -28.9 °C
12.7 ft-lb
@Thickness 0.125 in,
Temperature -20.0 °F
Geometry GC; ASTM D5420
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 93.3 °C200 °FISO 75-2/Bf
 105 °C221 °FUnannealed; ASTM D648
 119 °C246 °FAnnealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 54.4 °C130 °FISO 75-2/A

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Pro-fax PD702 Polypropylene Homopolymer, High Flow
ExxonMobil Achieve™ 6936G2 Polypropylene Homopolymer
Borealis Borflow™ HL508FB Polypropylene Homopolymer
ExxonMobil AP3AW Polypropylene Impact Copolymer
ExxonMobil PP4031E2 Polypropylene Impact Copolymer

PEX99438 / 175674

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.