MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Alliance BCN-10-2 Compression Bonded Neodymium Iron Boron Magnet
Categories: Ceramic; Oxide; Metal; Electronic/Magnetic Alloy

Material Notes: Compression Bonded Neodymium Iron Boron Magnets are made by utilizing the technique of compressing a “Rapid Spin Quenched” epoxy coated NdFeB magnet powder into a final shape and then heat treating it. The result is a high density material which produces a higher magnetic output than by injection molding. Although compression molding provides greater flexibility in geometry shape and size, it does not provide the range of complex geometries which can be achieved by injection molding.

Information provided by Alliance LLC.

Key Words: Permanent Magnet
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 5.60 - 6.00 g/cc0.202 - 0.217 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 80 - 12080 - 120
Modulus of Elasticity 28.0 GPa4060 ksi
Compressive Strength 27.0 - 33.0 MPa3920 - 4790 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0250 ohm-cm0.0250 ohm-cm
Magnetic Coercive Force, Hc 5400 - 5800 Oe5400 - 5800 Oe
 9800 - 10800 Oe9800 - 10800 OeIntrinsic
Magnetic Remanence, Br 6900 - 7100 Gauss6900 - 7100 Gauss
Magnetic Maximum Energy Product, BH 9.4 - 10.2 MGOe9.4 - 10.2 MGOe
Curie Temperature <= 310 °C<= 590 °F
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air <= 120 °C<= 248 °FLong term
 <= 160 °C<= 320 °FShort term
 
Descriptive Properties
Reversible Temperature Coefficients-0.13Bd. %/°C
 -0.4Hd. %/°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NALLIAN64b / 268394

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.