MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Thermal Ceramics Kao-Tuff 110C Castables
Categories: Ceramic; Oxide

Material Notes: Kao-Tuff 110C is a medium-weight erosion-resistant castable with excellent insulating properties. Abrasion losses 8 - 15 cc’s and a thermal conductivity of 5.5 at 1500°F (816°C) make it effective for numerous applications in F.C.C.U. and other industrial uses.

Features:

  • Feature specially enhanced properties that allow them to outperform conventional refractories
  • Abrasion losses from 8 to 22 cc’s
  • Gunning, hand packing and cast vibration placement techniques
  • Applications:

  • FCCU
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 1.667 - 1.827 g/ccFired at 1500°F
     1.683 - 1.811 g/ccFired at 2400°F
     
    Mechanical PropertiesOriginal ValueComments
    Modulus of Rupture 1.20 - 1.80 ksiDried 18-24 hours at 220°F; ASTM C133
     0.800 - 1.05 ksi
    @Treatment Temp. 816 °C,
    Time 18000 sec
    ASTM C133
     0.800 - 1.20 ksi
    @Treatment Temp. 1260 °C,
    Time 18000 sec
    ASTM C133
    Compressive Strength 37.9 - 58.6 MPaFired 5 hours at 1500°F; ASTM C133
     41.4 - 62.1 MPaDried for 18-24 hours at 220°F
     45.5 - 62.1 MPaFired 5 hours at 2400°F
     
    Thermal PropertiesOriginal ValueComments
    Thermal Conductivity 5.40 BTU-in/hr-ft²-°F
    @Temperature 260 °C
    ASTM C417
     5.40 BTU-in/hr-ft²-°F
    @Temperature 538 °C
    ASTM C417
     5.50 BTU-in/hr-ft²-°F
    @Temperature 816 °C
    ASTM C417
     5.70 BTU-in/hr-ft²-°F
    @Temperature 1090 °C
    ASTM C417
    Maximum Service Temperature, Air 2400 °F
    Shrinkage -0.400 - 0.40 %
    @Temperature 1320 °C,
    Time 18000 sec
    ASTM C113
     0.10 - 0.40 %
    @Temperature 816 °C,
    Time 18000 sec
    ASTM C113
     0.00 - 0.20 %
    @Treatment Temp. 104 °C
    Dried 18-24 hours; ASTM C113
     
    Processing PropertiesOriginal ValueComments
    Shelf Life 12.0 Month
     
    Component Elements PropertiesOriginal ValueComments
    Al2O3 43 %
    Alkalis 0.20 %
    CaO 15 %
    Fe2O3 1.8 %
    MgO 0.40 %
    SiO2 39 %
    TiO2 0.70 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Thermal Ceramics Kao-Tuff 110G Castables

    CTHERM065 / 2385

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.