Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.81 g/cc | 1.81 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Vickers | 80 - 105 | 80 - 105 |
Tensile Strength at Break | >= 240 MPa | >= 34800 psi |
| 169 MPa @Temperature 250 °C | 24500 psi @Temperature 482 °F |
| 191 MPa @Temperature 200 °C | 27700 psi @Temperature 392 °F |
| 211 MPa @Temperature 150 °C | 30600 psi @Temperature 302 °F |
| 230 MPa @Temperature 100 °C | 33400 psi @Temperature 212 °F |
| 261 MPa @Temperature 22.0 °C | 37900 psi @Temperature 71.6 °F |
Tensile Strength, Yield | >= 175 MPa @Strain 0.2 % | >= 25400 psi @Strain 0.2 % |
| 152 MPa @Strain 0.2 %, Temperature 250 °C | 22000 psi @Strain 0.2 %, Temperature 482 °F |
| 170 MPa @Strain 0.2 %, Temperature 200 °C | 24700 psi @Strain 0.2 %, Temperature 392 °F |
| 180 MPa @Strain 0.2 %, Temperature 150 °C | 26100 psi @Strain 0.2 %, Temperature 302 °F |
| 189 MPa @Strain 0.2 %, Temperature 100 °C | 27400 psi @Strain 0.2 %, Temperature 212 °F |
| 195 MPa @Strain 0.2 %, Temperature 22.0 °C | 28300 psi @Strain 0.2 %, Temperature 71.6 °F |
Elongation at Break | >= 2.0 % | >= 2.0 % |
| 4.0 % @Temperature 22.0 °C | 4.0 % @Temperature 71.6 °F |
| 10 % @Temperature 100 °C | 10 % @Temperature 212 °F |
| 15 % @Temperature 250 °C | 15 % @Temperature 482 °F |
| 16 % @Temperature 150 °C | 16 % @Temperature 302 °F |
| 16 % @Temperature 200 °C | 16 % @Temperature 392 °F |
Creep Strength | 17.0 MPa @Temperature 250 °C, Time 1.80e+6 sec | 2470 psi @Temperature 482 °F, Time 500 hour |
| 19.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 2760 psi @Temperature 482 °F, Time 1000 hour |
| 24.0 MPa @Temperature 250 °C, Time 3.60e+6 sec | 3480 psi @Temperature 482 °F, Time 1000 hour |
| 24.0 MPa @Temperature 250 °C, Time 1.80e+6 sec | 3480 psi @Temperature 482 °F, Time 500 hour |
| 29.0 MPa @Temperature 250 °C, Time 1.80e+6 sec | 4210 psi @Temperature 482 °F, Time 500 hour |
| 29.0 MPa @Temperature 250 °C, Time 360000 sec | 4210 psi @Temperature 482 °F, Time 100 hour |
| 36.0 MPa @Temperature 250 °C, Time 360000 sec | 5220 psi @Temperature 482 °F, Time 100 hour |
| 42.0 MPa @Temperature 250 °C, Time 360000 sec | 6090 psi @Temperature 482 °F, Time 100 hour |
| 46.0 MPa @Temperature 250 °C, Time 36000 sec | 6670 psi @Temperature 482 °F, Time 10.0 hour |
| 57.0 MPa @Temperature 200 °C, Time 1.80e+6 sec | 8270 psi @Temperature 392 °F, Time 500 hour |
| 62.0 MPa @Temperature 200 °C, Time 3.60e+6 sec | 8990 psi @Temperature 392 °F, Time 1000 hour |
| 73.0 MPa @Temperature 200 °C, Time 1.80e+6 sec | 10600 psi @Temperature 392 °F, Time 500 hour |
| 76.0 MPa @Temperature 200 °C, Time 3.60e+6 sec | 11000 psi @Temperature 392 °F, Time 1000 hour |
| 78.0 MPa @Temperature 200 °C, Time 360000 sec | 11300 psi @Temperature 392 °F, Time 100 hour |
| 88.0 MPa @Temperature 200 °C, Time 1.80e+6 sec | 12800 psi @Temperature 392 °F, Time 500 hour |
| 95.0 MPa @Temperature 200 °C, Time 360000 sec | 13800 psi @Temperature 392 °F, Time 100 hour |
| 109 MPa @Temperature 200 °C, Time 36000 sec | 15800 psi @Temperature 392 °F, Time 10.0 hour |
| 116 MPa @Temperature 200 °C, Time 360000 sec | 16800 psi @Temperature 392 °F, Time 100 hour |
| 123 MPa @Temperature 150 °C, Time 3.60e+6 sec | 17800 psi @Temperature 302 °F, Time 1000 hour |
| 128 MPa @Temperature 150 °C, Time 1.80e+6 sec | 18600 psi @Temperature 302 °F, Time 500 hour |
| 134 MPa @Temperature 150 °C, Time 3.60e+6 sec | 19400 psi @Temperature 302 °F, Time 1000 hour |
| 138 MPa @Temperature 150 °C, Time 360000 sec | 20000 psi @Temperature 302 °F, Time 100 hour |
| 140 MPa @Temperature 150 °C, Time 1.80e+6 sec | 20300 psi @Temperature 302 °F, Time 500 hour |
| 149 MPa @Temperature 150 °C, Time 36000 sec | 21600 psi @Temperature 302 °F, Time 10.0 hour |
| 152 MPa @Temperature 150 °C, Time 3.60e+6 sec | 22000 psi @Temperature 302 °F, Time 1000 hour |
| 155 MPa @Temperature 150 °C, Time 1.80e+6 sec | 22500 psi @Temperature 302 °F, Time 500 hour |
| 155 MPa @Temperature 150 °C, Time 360000 sec | 22500 psi @Temperature 302 °F, Time 100 hour |
Modulus of Elasticity | 44.0 GPa | 6380 ksi |
Compressive Yield Strength | 165 - 200 MPa @Strain 0.2 % | 23900 - 29000 psi @Strain 0.2 % |
Compressive Strength | 310 - 385 MPa | 45000 - 55800 psi |
Poissons Ratio | 0.30 | 0.30 |
Fatigue Strength | 60.0 - 70.0 MPa @# of Cycles 5.00e+7 | 8700 - 10200 psi @# of Cycles 5.00e+7 |
| 100 - 110 MPa @# of Cycles 5.00e+7 | 14500 - 16000 psi @# of Cycles 5.00e+7 |
Fracture Toughness | 16.4 MPa-m½ | 14.9 ksi-in½ |
Shear Strength | 152 MPa | 22000 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000685 ohm-cm | 0.00000685 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 26.7 µm/m-°C | 14.8 µin/in-°F |
Specific Heat Capacity | 1.00 J/g-°C | 0.239 BTU/lb-°F |
Thermal Conductivity | 113 W/m-K | 784 BTU-in/hr-ft²-°F |
Melting Point | 540 - 640 °C | 1000 - 1180 °F |
Solidus | 540 °C | 1000 °F |
Liquidus | 640 °C | 1180 °F |
Shrinkage | 1.3 % | 1.3 % |
|
Component Elements Properties | Metric | English | Comments |
---|
Copper, Cu | 0.050 - 0.10 % | 0.050 - 0.10 % |
Magnesium, Mg | 94.2 - 96.75 % | 94.2 - 96.75 % |
Rare Earths | 1.5 - 3.0 % | 1.5 - 3.0 % |
Silver, Ag | 1.3 - 1.7 % | 1.3 - 1.7 % |
Zirconium, Zr | 0.40 - 1.0 % | 0.40 - 1.0 % |
|
Descriptive Properties |
---|
Corrosion rate | 285 mpy |
Damping Index | 0.22 |