MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Alcoa QC-10® Aluminum Mold Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes: Specifically designed for high production injection and blow mold applications, QC-10 offers outstanding strength, stability, and durability. Its improved alloy composition provides outstanding, 1"- 24" thick section strength and hardness equal to that of rolled plate. Its quench insensitive microstructure allows minimal strength drop-off and excellent machinability.

Information provided by Alcoa.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.85 g/cc0.103 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 150 - 170150 - 170center
Tensile Strength, Ultimate  500 MPa
@Thickness >=508 mm
72500 psi
@Thickness >=20.0 in
at center (L/T direction)
 510 MPa
@Thickness 356 - 457 mm
74000 psi
@Thickness 14.0 - 18.0 in
at center (L/T direction)
 530 MPa
@Thickness 203 - 305 mm
76900 psi
@Thickness 8.00 - 12.0 in
at center (L/T direction)
 565 MPa
@Thickness 50.8 - 152 mm
81900 psi
@Thickness 2.00 - 6.00 in
at center (L/T direction)
Tensile Strength, Yield  455 MPa
@Thickness >=508 mm
66000 psi
@Thickness >=20.0 in
at center (L/T direction)
 470 MPa
@Thickness 356 - 457 mm
68200 psi
@Thickness 14.0 - 18.0 in
at center (L/T direction)
 500 MPa
@Thickness 203 - 305 mm
72500 psi
@Thickness 8.00 - 12.0 in
at center (L/T direction)
 525 MPa
@Thickness 50.8 - 152 mm
76100 psi
@Thickness 2.00 - 6.00 in
at center (L/T direction)
Elongation at Break  3.0 %
@Thickness >=508 mm
3.0 %
@Thickness >=20.0 in
at center (L/T direction)
 6.0 %
@Thickness 356 - 457 mm
6.0 %
@Thickness 14.0 - 18.0 in
at center (L/T direction)
 8.0 %
@Thickness 203 - 305 mm
8.0 %
@Thickness 8.00 - 12.0 in
at center (L/T direction)
 10 %
@Thickness 50.8 - 152 mm
10 %
@Thickness 2.00 - 6.00 in
at center (L/T direction)
Modulus of Elasticity 70.0 GPa10200 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 24.7 µm/m-°C13.7 µin/in-°F
Specific Heat Capacity 0.879 J/g-°C0.210 BTU/lb-°F
Thermal Conductivity 160 W/m-K1110 BTU-in/hr-ft²-°F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aleris Hokotol Aluminum Alloy, 100 mm Thickness
Aluminum 7075-T6; 7075-T651
Aluminum 201.0-T6 Casting Alloy
Overview of materials for Aluminum Casting Alloy
Alcoa MIC-6 Aluminum Mold Alloy

NALCOA90 / 10263

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.