MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Crucible Steel CPM® 4V® Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel

Material Notes: CPM 4V is a powder metal tool steel with an outstanding combination of properties including high impact toughness and very good wear resistance. CPM 4V should be considered for service in fine blanking, powder compaction tools, for processing high-strength low-alloy (HSLA) steels, advanced high-strength steels (AHSS) and applications where a combination of strength , wear resistance and toughness is required.

CPM 4V should be considered for applications where a higher attainable hardness and additional abrasion resistance is required than can be offered by CPM 3V.

Information provided by Crucible Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.70 g/cc0.278 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  >= 44
@Tempering Temp. 621 °C
>= 44
@Tempering Temp. 1150 °F
austenitized at 1800°F, then quenched and tempered
 50
@Tempering Temp. 621 °C
50
@Tempering Temp. 1150 °F
austenitized at 1950°F, then quenched and tempered
 55
@Tempering Temp. 593 °C
55
@Tempering Temp. 1100 °F
austenitized at 1950°F, then quenched and tempered
 60
@Tempering Temp. 566 °C
60
@Tempering Temp. 1050 °F
austenitized at 1950°F, then quenched and tempered
 62
@Tempering Temp. 538 °C
62
@Tempering Temp. 1000 °F
austenitized at 1950°F, then quenched and tempered
 <= 64
@Tempering Temp. 538 °C
<= 64
@Tempering Temp. 1000 °F
austenitized at 2100°F, then quenched and tempered
Modulus of Elasticity 207 GPa30000 ksi
Charpy Impact  48.8 J
@Treatment Temp. 1120 °C
36.0 ft-lb
@Treatment Temp. 2050 °F
austenitized; C-notch
 67.8 J
@Treatment Temp. 1070 °C
50.0 ft-lb
@Treatment Temp. 1950 °F
austenitized; C-notch
 74.6 J
@Treatment Temp. 982 °C
55.0 ft-lb
@Treatment Temp. 1800 °F
austenitized; C-notch
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.460 J/g-°C0.110 BTU/lb-°F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 1.35 %1.35 %
Chromium, Cr 5.0 %5.0 %
Iron, Fe 85.65 %85.65 %as balance
Manganese, Mn 0.40 %0.40 %
Molybdenum, Mo 2.95 %2.95 %
Silicon, Si 0.80 %0.80 %
Vanadium, V 3.85 %3.85 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Crucible Steel CPM® Rex M4 HC(HS) Tool Steel
ASTM A709 Steel, grade 100 and 100W, > 64 mm & < 100 mm
Crucible Steel CPM® 3V® Tool Steel
AISI Type M4 Molybdenum High Speed Tool Steel (UNS T11304)
Crucible Steel REX® M4 High Speed Steel

NCRUC905 / 160356

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.