Physical Properties | Metric | English | Comments |
---|
Density | 1.55 g/cc | 0.0560 lb/in³ |
Moisture Absorption | 1.80 % | 1.80 % |
Linear Mold Shrinkage, Flow | 0.0035 cm/cm | 0.0035 in/in |
Linear Mold Shrinkage, Transverse | 0.010 cm/cm | 0.010 in/in |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 78.0 MPa @Temperature 200 °C | 11300 psi @Temperature 392 °F |
| 85.0 MPa @Temperature 180 °C | 12300 psi @Temperature 356 °F |
| 90.0 MPa @Temperature 120 °C | 13100 psi @Temperature 248 °F |
| 95.0 MPa @Temperature 160 °C | 13800 psi @Temperature 320 °F |
| 100 MPa @Temperature 100 °C | 14500 psi @Temperature 212 °F |
| 105 MPa @Temperature 150 °C | 15200 psi @Temperature 302 °F |
| 115 MPa @Temperature 80.0 °C | 16700 psi @Temperature 176 °F |
| 140 MPa @Temperature 120 °C | 20300 psi @Temperature 248 °F |
| 170 MPa @Temperature 100 °C | 24700 psi @Temperature 212 °F |
| 190 MPa @Temperature 40.0 °C | 27600 psi @Temperature 104 °F |
| 200 MPa @Temperature 80.0 °C | 29000 psi @Temperature 176 °F |
| 210 MPa @Temperature 23.0 °C | 30500 psi @Temperature 73.4 °F |
| 220 MPa @Temperature 40.0 °C | 31900 psi @Temperature 104 °F |
| 230 MPa @Temperature 23.0 °C | 33400 psi @Temperature 73.4 °F |
| 250 MPa @Temperature -40.0 °C | 36300 psi @Temperature -40.0 °F |
| 250 MPa @Temperature -40.0 °C | 36300 psi @Temperature -40.0 °F |
Elongation at Break | 2.1 % @Temperature -40.0 °C | 2.1 % @Temperature -40.0 °F |
| 2.1 % @Temperature 40.0 °C | 2.1 % @Temperature 104 °F |
| 2.2 % @Temperature 23.0 °C | 2.2 % @Temperature 73.4 °F |
| 2.2 % @Temperature -40.0 °C | 2.2 % @Temperature -40.0 °F |
| 2.2 % @Temperature 40.0 °C | 2.2 % @Temperature 104 °F |
| 2.3 % @Temperature 23.0 °C | 2.3 % @Temperature 73.4 °F |
| 2.5 % @Temperature 80.0 °C | 2.5 % @Temperature 176 °F |
| 3.0 % @Temperature 100 °C | 3.0 % @Temperature 212 °F |
| 4.5 % @Temperature 80.0 °C | 4.5 % @Temperature 176 °F |
| 5.0 % @Temperature 100 °C | 5.0 % @Temperature 212 °F |
| 5.1 % @Temperature 120 °C | 5.1 % @Temperature 248 °F |
| 6.0 % @Temperature 120 °C | 6.0 % @Temperature 248 °F |
| 6.9 % @Temperature 150 °C | 6.9 % @Temperature 302 °F |
| 7.0 % @Temperature 160 °C | 7.0 % @Temperature 320 °F |
| 7.0 % @Temperature 180 °C | 7.0 % @Temperature 356 °F |
| 7.0 % @Temperature 200 °C | 7.0 % @Temperature 392 °F |
Tensile Modulus | 5.30 GPa @Temperature 200 °C | 769 ksi @Temperature 392 °F |
| 5.50 GPa @Temperature 180 °C | 798 ksi @Temperature 356 °F |
| 6.30 GPa @Temperature 120 °C | 914 ksi @Temperature 248 °F |
| 6.30 GPa @Temperature 160 °C | 914 ksi @Temperature 320 °F |
| 6.70 GPa @Temperature 150 °C | 972 ksi @Temperature 302 °F |
| 7.00 GPa @Temperature 100 °C | 1020 ksi @Temperature 212 °F |
| 8.80 GPa @Temperature 80.0 °C | 1280 ksi @Temperature 176 °F |
| 9.50 GPa @Temperature 120 °C | 1380 ksi @Temperature 248 °F |
| 12.8 GPa @Temperature 100 °C | 1860 ksi @Temperature 212 °F |
| 13.5 GPa @Temperature 80.0 °C | 1960 ksi @Temperature 176 °F |
| 14.0 GPa @Temperature 40.0 °C | 2030 ksi @Temperature 104 °F |
| 14.2 GPa @Temperature 40.0 °C | 2060 ksi @Temperature 104 °F |
| 14.5 GPa @Temperature 23.0 °C | 2100 ksi @Temperature 73.4 °F |
| 14.8 GPa @Temperature 23.0 °C | 2150 ksi @Temperature 73.4 °F |
| 14.8 GPa @Temperature -40.0 °C | 2150 ksi @Temperature -40.0 °F |
| 15.0 GPa @Temperature -40.0 °C | 2180 ksi @Temperature -40.0 °F |
Flexural Strength | 290 MPa | 42100 psi |
| 350 MPa | 50800 psi |
Flexural Modulus | 5.00 GPa @Temperature 200 °C | 725 ksi @Temperature 392 °F |
| 5.40 GPa @Temperature 180 °C | 783 ksi @Temperature 356 °F |
| 6.00 GPa @Temperature 160 °C | 870 ksi @Temperature 320 °F |
| 9.80 GPa @Temperature 120 °C | 1420 ksi @Temperature 248 °F |
| 14.0 GPa @Temperature 23.0 °C | 2030 ksi @Temperature 73.4 °F |
| 14.5 GPa @Temperature 23.0 °C | 2100 ksi @Temperature 73.4 °F |
Fatigue Strength | 100 MPa @# of Cycles 316 , Temperature 140 °C | 14500 psi @# of Cycles 316 , Temperature 284 °F |
Charpy Impact Unnotched | 5.50 J/cm² @Temperature -30.0 °C | 26.2 ft-lb/in² @Temperature -22.0 °F |
| 6.00 J/cm² @Temperature 23.0 °C | 28.6 ft-lb/in² @Temperature 73.4 °F |
| 6.50 J/cm² @Temperature -30.0 °C | 30.9 ft-lb/in² @Temperature -22.0 °F |
| 7.00 J/cm² @Temperature 23.0 °C | 33.3 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 0.800 J/cm² @Temperature -30.0 °C | 3.81 ft-lb/in² @Temperature -22.0 °F |
| 0.900 J/cm² @Temperature 23.0 °C | 4.28 ft-lb/in² @Temperature 73.4 °F |
| 1.00 J/cm² @Temperature -30.0 °C | 4.76 ft-lb/in² @Temperature -22.0 °F |
| 1.10 J/cm² @Temperature 23.0 °C | 5.23 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | >= 1.00e+13 ohm-cm | >= 1.00e+13 ohm-cm |
| >= 1.00e+13 ohm-cm | >= 1.00e+13 ohm-cm |
Dielectric Constant | 4.6 @Frequency 1e+6 Hz | 4.6 @Frequency 1e+6 Hz |
| 4.8 @Frequency 1e+6 Hz | 4.8 @Frequency 1e+6 Hz |
| 4.9 @Frequency 100 Hz | 4.9 @Frequency 100 Hz |
| 5.7 @Frequency 100 Hz | 5.7 @Frequency 100 Hz |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 35.0 µm/m-°C | 19.4 µin/in-°F |
CTE, linear, Parallel to Flow | 30.0 µm/m-°C | 16.7 µin/in-°F |
Melting Point | 325 °C | 617 °F |
Maximum Service Temperature, Air | 175 °C | 347 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 305 °C | 581 °F |