MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polyether Block Amide (PEBA)
Categories: Polymer; Thermoplastic; Polyether Block Amide (PEBA)

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyether Block Amide (PEBA)". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.870 - 11.0 g/cc0.0314 - 0.397 lb/in³Average value: 1.32 g/cc Grade Count:83
 0.830 - 0.830 g/cc
@Temperature 200 - 260 °C
0.0300 - 0.0300 lb/in³
@Temperature 392 - 500 °F
Average value: 0.830 g/cc Grade Count:7
Water Absorption 0.700 - 120 %0.700 - 120 %Average value: 10.1 % Grade Count:46
Moisture Absorption at Equilibrium 0.400 - 4.50 %0.400 - 4.50 %Average value: 0.951 % Grade Count:47
Water Absorption at Saturation 1.00 - 1.50 %1.00 - 1.50 %Average value: 1.20 % Grade Count:6
Viscosity Number 190 cm³/g1.90 dl/gAverage value: 190 cm³/g Grade Count:5
Linear Mold Shrinkage 0.00200 - 0.0150 cm/cm0.00200 - 0.0150 in/inAverage value: 0.00921 cm/cm Grade Count:48
Linear Mold Shrinkage, Transverse 0.00400 - 0.0150 cm/cm0.00400 - 0.0150 in/inAverage value: 0.00862 cm/cm Grade Count:12
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 75.0 - 92.075.0 - 92.0Average value: 84.5 Grade Count:13
Hardness, Shore D 22.0 - 73.022.0 - 73.0Average value: 49.1 Grade Count:59
Tensile Strength, Ultimate 9.00 - 140 MPa1310 - 20300 psiAverage value: 48.0 MPa Grade Count:44
Tensile Strength, Yield 6.89 - 43.0 MPa999 - 6240 psiAverage value: 19.6 MPa Grade Count:32
Film Elongation at Break, MD 500 %500 %Average value: 500 % Grade Count:4
Film Elongation at Break, TD 600 - 700 %600 - 700 %Average value: 675 % Grade Count:4
Elongation at Break 1.00 - 1000 %1.00 - 1000 %Average value: 110 % Grade Count:75
Elongation at Yield 5.10 - 42.0 %5.10 - 42.0 %Average value: 24.6 % Grade Count:31
Modulus of Elasticity 0.0100 - 11.0 GPa1.45 - 1600 ksiAverage value: 0.880 GPa Grade Count:72
Flexural Yield Strength 12.0 - 165 MPa1740 - 23900 psiAverage value: 78.6 MPa Grade Count:14
Flexural Modulus 0.200 - 10.0 GPa29.0 - 1450 ksiAverage value: 3.68 GPa Grade Count:18
Izod Impact, Notched 0.530 - 5340 J/cm0.993 - 10000 ft-lb/inAverage value: 1.42 J/cm Grade Count:4
Izod Impact, Notched (ISO) 10.0 - 50.0 kJ/m²4.76 - 23.8 ft-lb/in²Average value: 31.8 kJ/m² Grade Count:11
 5.00 - 46.0 kJ/m²
@Temperature -30.0 - -30.0 °C
2.38 - 21.9 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 22.2 kJ/m² Grade Count:11
Izod Impact, Unnotched (ISO) 5.25 - 155 kJ/m²2.50 - 73.8 ft-lb/in²Average value: 96.2 kJ/m² Grade Count:12
 68.0 - 120 kJ/m²
@Temperature -30.0 - -30.0 °C
32.4 - 57.1 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 90.6 kJ/m² Grade Count:11
Charpy Impact Unnotched 1000 J/cm² - NB4760 ft-lb/in² - NBGrade Count:57
 999.9 J/cm² - NB
@Temperature -30.0 - -30.0 °C
4759 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Grade Count:57
Charpy Impact, Notched 0.800 J/cm² - NB3.81 ft-lb/in² - NBAverage value: 6.09 J/cm² Grade Count:57
 0.400 J/cm² - NB
@Temperature -30.0 - -30.0 °C
1.90 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 1.63 J/cm² Grade Count:56
Tensile Creep Modulus, 1000 hours 60.0 - 200 MPa8700 - 29000 psiAverage value: 113 MPa Grade Count:4
Tear Strength 44.0 - 166 kN/m251 - 947 pliAverage value: 96.2 kN/m Grade Count:9
Compression Set 19.0 - 47.0 %19.0 - 47.0 %Average value: 33.3 % Grade Count:6
Film Tensile Strength at Break, MD 0.365 - 32.0 MPa53.0 - 4640 psiAverage value: 24.1 MPa Grade Count:4
Film Tensile Strength at Break, TD 34.0 MPa4930 psiAverage value: 34.0 MPa Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00500 - 9.00e+13 ohm-cm0.00500 - 9.00e+13 ohm-cmAverage value: 7.93e+12 ohm-cm Grade Count:31
Surface Resistance 0.200 - 1.84e+14 ohm0.200 - 1.84e+14 ohmAverage value: 1.15e+13 ohm Grade Count:34
Dielectric Constant 4.00 - 13.04.00 - 13.0Average value: 6.51 Grade Count:15
Dielectric Strength 5.00 - 44.5 kV/mm127 - 1130 kV/inAverage value: 32.0 kV/mm Grade Count:18
Dissipation Factor 0.0310 - 0.6260.0310 - 0.626Average value: 0.119 Grade Count:15
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:15
 
Thermal PropertiesMetricEnglishComments
CTE, linear 100 - 240 µm/m-°C55.6 - 133 µin/in-°FAverage value: 179 µm/m-°C Grade Count:17
CTE, linear, Transverse to Flow 100 - 210 µm/m-°C55.6 - 117 µin/in-°FAverage value: 169 µm/m-°C Grade Count:7
Specific Heat Capacity 2.50 - 2.80 J/g-°C0.598 - 0.669 BTU/lb-°FAverage value: 2.74 J/g-°C Grade Count:7
Thermal Conductivity 0.180 - 0.200 W/m-K
@Temperature 200 - 260 °C
1.25 - 1.39 BTU-in/hr-ft²-°F
@Temperature 392 - 500 °F
Average value: 0.183 W/m-K Grade Count:7
Melting Point 134 - 218 °C273 - 424 °FAverage value: 168 °C Grade Count:59
Deflection Temperature at 0.46 MPa (66 psi) 42.0 - 165 °C108 - 329 °FAverage value: 88.3 °C Grade Count:22
Deflection Temperature at 1.8 MPa (264 psi) 45.0 - 155 °C113 - 311 °FAverage value: 84.4 °C Grade Count:11
Deflection Temperature at 8.0 MPa 55.0 - 110 °C131 - 230 °FAverage value: 90.0 °C Grade Count:5
Vicat Softening Point 58.0 - 175 °C136 - 347 °FAverage value: 133 °C Grade Count:48
Glass Transition Temp, Tg -65.0 - -40.0 °C-85.0 - -40.0 °FAverage value: -50.7 °C Grade Count:7
Flammability, UL94 HBHBGrade Count:10
Oxygen Index 19.0 - 23.0 %19.0 - 23.0 %Average value: 20.0 % Grade Count:5
 
Processing PropertiesMetricEnglishComments
Melt Temperature 180 - 271 °C356 - 520 °FAverage value: 241 °C Grade Count:67
Mold Temperature 10.0 - 82.2 °C50.0 - 180 °FAverage value: 40.5 °C Grade Count:66
Injection Velocity 200 mm/sec7.87 in/secAverage value: 200 mm/sec Grade Count:14
Drying Temperature 55.0 - 100 °C131 - 212 °FAverage value: 83.7 °C Grade Count:16

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Styrenic Elastomer (TES)
Overview of materials for Polyester Thermoplastic Elastomer
Overview of materials for Thermoplastic Olefinic Elastomer (TPO)
Overview of materials for Silicone Rubber
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade

O5460 / 77785

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.