  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Titanium Ti-10V-2Fe-3Al (Ti 10-2-3), Anneal 1 hr. 760°C
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Excellent mechanical properties up to 315 °C. High strength and high toughness. Deep hardenability, excellent creep stability, excellent forgability.

Applications: Airframe applications, milling, forgings

Forms typically available: Billet, bar and plate

5 other heat treatments of this alloy are in MatWeb.

Key Words: KS 10-2-3; Ti 10-2-3; TIMETAL 10-2-3
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.65 g/cc0.168 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 304304Estimated from Rockwell C.
Hardness, Knoop 330330Estimated from Rockwell C.
Hardness, Rockwell C 3232
Hardness, Vickers 318318Estimated from Rockwell C.
Tensile Strength, Ultimate 970 MPa141000 psi
Tensile Strength, Yield 900 MPa131000 psi
Elongation at Break 9.0 %9.0 %
Modulus of Elasticity 110 GPa16000 ksiAfter aging.
Poissons Ratio 0.330.33Typical for beta titanium alloy.
Shear Modulus 41.0 GPa5950 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000150 ohm-cm0.000150 ohm-cmEstimated from similar high-V-stabilized beta titanium alloys.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.70 µm/m-°C
@Temperature 20.0 - 100 °C
5.39 µin/in-°F
@Temperature 68.0 - 212 °F
 9.70 µm/m-°C
@Temperature 20.0 - 425 °C
5.39 µin/in-°F
@Temperature 68.0 - 797 °F
average
Specific Heat Capacity 0.525 J/g-°C0.125 BTU/lb-°FTypical value for titanium alloys.
Thermal Conductivity 7.80 W/m-K54.1 BTU-in/hr-ft²-°FEstimated from similar high-V-stabilized beta titanium alloys.
Maximum Service Temperature, Air 315 °C599 °F
Beta Transus 760 °C1400 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 2.6 - 3.4 %2.6 - 3.4 %
Carbon, C <= 0.050 %<= 0.050 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe 1.6 - 2.2 %1.6 - 2.2 %
Nitrogen, N <= 0.050 %<= 0.050 %
Other, each <= 0.10 %<= 0.10 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.13 %<= 0.13 %
Titanium, Ti 82.855 - 86.8 %82.855 - 86.8 %As Balance; Elemental Composition per ASTM B265
Vanadium, V 9.0 - 11 %9.0 - 11 %
 
Descriptive Properties
Crystal StructurebccBeta, predominant
 cphAlpha

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C, Aged 385°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) Solution Treated 850°C (1560°F)
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C; Age 525°C (980°F)
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 730°C; overage 580°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 815°C, Anneal 620°C

MTB025 / 14149

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.