American Longleaf Pine Wood
Categories: Wood and Natural Products; Wood; Softwood

Material Notes: Softwood. Relatively easy to work with hand tools. Data is based on small, clear, air-dried samples unless specified.

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Pinus palustris; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.550 g/cc0.0199 lb/in³Oven Dry Weight/Unseasoned Volume
 0.657 g/cc0.0237 lb/in³Unseasoned*
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 2400 N540 lb (f)End. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 2600 N585 lb (f)Side. Force required to imbed a 0.444 inch steel ball to one-half its diameter
Tensile Strength, Ultimate 2.00 MPa290 psiPerpendicular to Grain*
Modulus of Rupture 0.0600 GPa8.70 ksiStatic Bending*
 0.101 GPa14.6 ksiIn Bending
Flexural Yield Strength 37.2 MPa5400 psiFiber Stress at Elastic Limit; Static Bending*
 64.1 MPa9300 psiBending stress at proportional limit
Flexural Modulus 11.2 GPa1630 ksiStatic Bending*
 13.8 GPa2000 ksiIn Bending
Compressive Strength 4.14 MPa600 psiPerpendicular to Grain*
 19.6 MPa2840 psiParallel to Grain*
 30.3 MPa4390 psiMax Crushing Strength Parallel to Grain*
 57.9 - 58.6 MPa8400 - 8500 psiParallel to Grain
Poissons Ratio 0.3320.332µLR, 12% Moisture Content
 0.3420.342µTR, 12% Moisture Content
 0.3650.365µLT, 12% Moisture Content
 0.3840.384µRT, 12% Moisture Content
Shear Strength 7.38 MPa1070 psiParallel to Grain*
 10.3 MPa1490 psiOrientation Unknown
Impact 3.53.5in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 1080010800psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.00689 J/cm³1.00 in-lb/in³Static Bending*
Work to Maximum Load 0.0552 J/cm³8.00 in-lb/in³Static Bending*
Cleavage 32.0 kN/m183 lb/inTangential surface of failure, Unseasoned*
 33.0 kN/m188 lb/inRadial surface of failure, Unseasoned*
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.138 W/m-K0.960 BTU-in/hr-ft²-°FOven Dry
 0.173 W/m-K1.20 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 5.3 %5.3 %Radial; Unseasoned to Oven Dry*
 7.5 %7.5 %Tangential; Unseasoned to Oven Dry*
 12.4 %12.4 %Volumetric; Unseasoned to Oven Dry*

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.