Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Applications include pipe, railings, furniture, architectural extrusions, irrigation pipes, and transportation.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96063; ISO AlMg0.5Si; Aluminium 6063-T6; AA6063-T6; Al6063-T6
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.70 g/cc0.0975 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 7373AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 9696Converted from Brinell Hardness Value
Hardness, Vickers 8383Converted from Brinell Hardness Value
Tensile Strength, Ultimate 241 MPa35000 psiAA; Typical
 16.0 MPa
@Temperature 371 °C
2320 psi
@Temperature 700 °F
 23.0 MPa
@Temperature 316 °C
3340 psi
@Temperature 601 °F
 31.0 MPa
@Temperature 260 °C
4500 psi
@Temperature 500 °F
 62.0 MPa
@Temperature 204 °C
8990 psi
@Temperature 399 °F
 145 MPa
@Temperature 149 °C
21000 psi
@Temperature 300 °F
 214 MPa
@Temperature 100 °C
31000 psi
@Temperature 212 °F
 241 MPa
@Temperature 24.0 °C
35000 psi
@Temperature 75.2 °F
 248 MPa
@Temperature -28.0 °C
36000 psi
@Temperature -18.4 °F
 262 MPa
@Temperature -80.0 °C
38000 psi
@Temperature -112 °F
 324 MPa
@Temperature -196 °C
47000 psi
@Temperature -321 °F
Tensile Strength, Yield 214 MPa31000 psiAA; Typical
 14.0 MPa
@Strain 0.2 %,
Temperature 371 °C
2030 psi
@Strain 0.2 %,
Temperature 700 °F
 17.0 MPa
@Strain 0.2 %,
Temperature 316 °C
2470 psi
@Strain 0.2 %,
Temperature 601 °F
 24.0 MPa
@Strain 0.2 %,
Temperature 260 °C
3480 psi
@Strain 0.2 %,
Temperature 500 °F
 45.0 MPa
@Strain 0.2 %,
Temperature 204 °C
6530 psi
@Strain 0.2 %,
Temperature 399 °F
 133 MPa
@Strain 0.2 %,
Temperature 149 °C
19300 psi
@Strain 0.2 %,
Temperature 300 °F
 193 MPa
@Strain 0.2 %,
Temperature 100 °C
28000 psi
@Strain 0.2 %,
Temperature 212 °F
 214 MPa
@Strain 0.2 %,
Temperature 24.0 °C
31000 psi
@Strain 0.2 %,
Temperature 75.2 °F
 221 MPa
@Strain 0.2 %,
Temperature -28.0 °C
32100 psi
@Strain 0.2 %,
Temperature -18.4 °F
 228 MPa
@Strain 0.2 %,
Temperature -80.0 °C
33100 psi
@Strain 0.2 %,
Temperature -112 °F
 248 MPa
@Strain 0.2 %,
Temperature -196 °C
36000 psi
@Strain 0.2 %,
Temperature -321 °F
Elongation at Break  15 %
@Temperature 100 °C
15 %
@Temperature 212 °F
 18 %
@Temperature 24.0 °C
18 %
@Temperature 75.2 °F
 19 %
@Temperature -28.0 °C
19 %
@Temperature -18.4 °F
 20 %
@Temperature -80.0 °C
20 %
@Temperature -112 °F
 20 %
@Temperature 149 °C
20 %
@Temperature 300 °F
 24 %
@Temperature -196 °C
24 %
@Temperature -321 °F
 40 %
@Temperature 204 °C
40 %
@Temperature 399 °F
 75 %
@Temperature 260 °C
75 %
@Temperature 500 °F
 80 %
@Temperature 316 °C
80 %
@Temperature 601 °F
 105 %
@Temperature 371 °C
105 %
@Temperature 700 °F
 12 %
@Thickness 1.59 mm
12 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Ultimate Bearing Strength 434 MPa62900 psiEdge distance/pin diameter = 2.0
Bearing Yield Strength 276 MPa40000 psiEdge distance/pin diameter = 2.0
Poissons Ratio 0.330.33
Fatigue Strength 68.9 MPa
@# of Cycles 5.00e+8
10000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 50 %50 %0-100 Scale of Aluminum Alloys
Shear Modulus 25.8 GPa3740 ksi
Shear Strength 152 MPa22000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000332 ohm-cm
@Temperature 20.0 °C
0.00000332 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
13.0 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.5 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.6 µm/m-°C
@Temperature 20.0 - 300 °C
14.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°F
Thermal Conductivity 200 W/m-K1390 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 616 - 654 °C1140 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 616 °C1140 °FAA; Typical
Liquidus 654 °C1210 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °Fhold at temperature for 2 to 3 hr; cool at 50°F per hour from 775 to 500°F
Solution Temperature 521 °C970 °F
Aging Temperature 177 °C350 °Fhold at temperature for 8 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 97.5 %<= 97.5 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.35 %<= 0.35 %
Magnesium, Mg 0.45 - 0.90 %0.45 - 0.90 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.20 - 0.60 %0.20 - 0.60 %
Titanium, Ti <= 0.10 %<= 0.10 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.