American Eastern White Pine Wood
Categories: Wood and Natural Products; Wood; Softwood

Material Notes: Softwood. Easy to work with hand tools. Data is based on small, clear, air-dried samples unless specified.

Key Words: Pinus strobus; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.350 g/cc0.0126 lb/in³Air Dry (12-15% Moisture Content)
Cell Length 3.00 mm0.118 inMature Wood
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 1700 N382 lb (f)Side
Tensile Strength, Ultimate 2.10 MPa305 psiPerpendicular to Grain
 78.0 MPa11300 psiAxial
Modulus of Rupture 0.0590 GPa8.56 ksiIn Bending
Flexural Yield Strength 41.4 MPa6000 psiBending stress at proportional limit
Flexural Modulus 8.30 - 8.56 GPa1200 - 1240 ksiIn Bending
Compressive Strength 3.50 MPa508 psiPerpendicular to Grain
 33.0 - 33.1 MPa4790 - 4800 psiParallel to Grain
Shear Strength 6.20 MPa899 psiOrientation Unknown
Toughness 12.4 J9.15 ft-lbRadial
 13.6 J10.0 ft-lbTangential
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0908 W/m-K0.630 BTU-in/hr-ft²-°FOven Dry
 0.108 W/m-K0.750 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 2.3 %2.3 %Radial; Green to Zero Moisture
 6.0 %6.0 %Tangential; Green to Zero Moisture
 8.2 %8.2 %Volumetric; Green to Zero Moisture

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.