MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
SABIC LNP™ THERMOCOMP™ HF008 Nylon 11 (Global)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 11 (PA11)

Material Notes: LNP THERMOCOMP* HF008 is a compound based on Nylon 11 resin containing 40% Glass Fiber.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccASTM D792
 1.37 g/ccISO 1183
Moisture Absorption 0.100 %50% RH, 24 hrs; ASTM D570
 0.190 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cm24HRS; ASTM D955
 0.0010 - 0.0030 cm/cm24HRS; ISO 294
Linear Mold Shrinkage, Transverse 0.0080 - 0.010 cm/cm24 HRS; ASTM D955
 0.0080 - 0.010 cm/cm24 HRS; ISO 294
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 122 MPaASTM D638
 123 MPaISO 527
Elongation at Break 3.9 %ISO 527
 4.9 %ASTM D638
Tensile Modulus 7600 MPa1 mm/min; ISO 527
 9280 MPa50 mm/min; ASTM D638
Flexural Strength 192 MPaISO 178
 220 MPaASTM D790
Flexural Modulus 7970 MPaISO 178
 8480 MPaASTM D790
Izod Impact, Notched 240 J/mASTM D256
Izod Impact, Unnotched 1228 J/mASTM D4812
Izod Impact, Notched (ISO) 21.0 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 75.0 kJ/m²80*10*4; ISO 180/1U
Impact Test 3.00 JMultiaxial Impact; ISO 6603
Instrumented Impact Energy at Peak 18.0 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 28.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 30.4 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 88.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 88.7 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 175 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 177 °C
@Thickness 3.20 mm
unannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Zone 1 200 - 210 °C
Zone 2 230 - 245 °CInjection Molding
Zone 3 260 - 270 °C
Melt Temperature 225 - 260 °CInjection Molding
Mold Temperature 45.0 - 55.0 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Moisture Content 0.15 %Injection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH92209 / 253333

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.