MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
UBE Upilex® 50S Polyimide Film
Categories: Polymer; Thermoset; Polyimide, TS; Polyimide, Thermoset Film

Material Notes: Polyimide resin combining high heat resistance, chemical resistance, etc. is widely adopted for electronic equipment and so on. Films, varnishes and many other products are available. Compared to other polyimide films, it has better surface smoothness and higher chemical resistance, greater stiffness and much higher heat resistance. Out gassing is very low, so it is easy to use. UPILEX®-S" delivers outstanding mechanical characteristics across a wide temperature range. It also demonstrates high tensile strength and modulus, and even features outstanding long-term heat resistance. Another exceptional feature of "UPILEX®-S" is its high resistance to hydrolysis, as demonstrated by its properties being virtually unaffected even when it is immersed in boiling water for long periods of time.

Information provided by UBE Industries, LTD

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.47 g/cc
@Temperature 25.0 °C
ASTM D1505
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 290 MPa
@Temperature 300 °C
ASTM D882
 460 MPa
@Temperature 25.0 °C
ASTM D882
Elongation at Break 50 %
@Temperature 25.0 °C
ASTM D882
 70 %
@Temperature 300 °C
ASTM D882
Tensile Modulus 3.70 GPa
@Temperature 300 °C
ASTM D882
 9.30 GPa
@Temperature 25.0 °C
ASTM D882
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.0 µm/m-°C
@Temperature 50.0 - 200 °C
Fine linear dilatometer 5°C/min.
Specific Heat Capacity 1.13 J/g-°CDifferential scanning calorimeter
Maximum Service Temperature, Air 290 °CTensile Strength. 20,000hr heat life
Flammability, UL94 V-0
Oxygen Index 66 %JIS K7201
Shrinkage 0.020 %
@Temperature 200 °C,
Time 7200 sec
heat; ASTM D1204
 
Descriptive Properties
Surface Roughness (nm)1.2Ra. Scanning probe microscope area = 10mm x 10mm. General Polyimide=3.2. PET=22
 2Rms. Scanning probe microscope area = 10mm x 10mm
 60.3Rz. Scanning probe microscope area = 10mm x 10mm. General Polyimide=100

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PUBD9847 / 287310

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.