MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Ravago Manufacturing Americas Hylex® P1007L Polycarbonate  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes:

Information provided by Ravago

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccASTM D792
Water Absorption 0.15 %24 hrs; ASTM D570
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cmASTM D955
Melt Flow 7.0 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 80ASTM D785
Tensile Strength at Break 10100 psiASTM D638
Elongation at Break 130 %ASTM D638
Flexural Strength 13500 psiASTM D790
Flexural Modulus 340000 psiASTM D790
Izod Impact, Notched 17.0 ft-lb/in73°F, 0.125 in; ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.00e+16 ohm-cmASTM D257
Dielectric Strength 410 V/milin Air, 0.125 in; ASTM D149
Arc Resistance 120 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 285 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 270 °FUnannealed; ASTM D648
Vicat Softening Point 310 °FASTM D1525
Flammability, UL94 HB
@Thickness 1.47 mm
natural color
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.585ASTM D542
Haze 0.50 - 0.80 %
@Thickness 3.17 mm
ASTM D1003
Transmission, Visible 89 - 91 %ASTM D1003
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 540 - 580 °F
Middle Barrel Temperature 550 - 590 °F
Front Barrel Temperature 590 - 630 °F
Nozzle Temperature 570 - 620 °F
Melt Temperature 590 - 640 °F
Mold Temperature 180 - 230 °F
Drying Temperature 250 °F
Dry Time 3 - 12 hour
Moisture Content <= 0.020 %
Injection Pressure 1500 - 2000 psi
Back Pressure 70.0 - 150 psi
Shot Size 40 - 60 %
Screw Speed 40 - 70 rpm
 
Descriptive Properties
Holding Pressure1000 to 1400 psi

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PENTA033 / 36043

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.