MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Daikin DAI-EL® G-801 Fluoroelastomer Terpolymer, 66% Fluorine Content
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: DAI-EL® G-801 is a peroxide curable copolymer with medium Mooney viscosity suitable for transfer and compression molding. DAI-EL® G-801can be formulated with various peroxide cure systems to eliminate the need for post cure. DAI-EL® G-801 provides superior mechanical properties and resistance to steam and aqueous solvents compared with bisphenol cured fluoroelastomers. DAI-EL® G-801 may be used in compliance with 21 CFR 177.2600, Rubber articles intended for repeated use. Finished articles are required to comply with the end tests specified in 21 CFR 177.2600 (e) or (f), as applicable.

Typical Applications: O-Rings, gaskets, seals

Rheological Properties MDR 2000:
Temperature: 177°C
Frequency: 100 cpm
Strain: 0.5°
Test time: 6 min

Information provided by Daikin.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.81 g/cc1.81 g/cc
Mooney Viscosity 37
@Temperature 121 °C
37
@Temperature 250 °F
ML 1+10
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7171
Tensile Strength at Break 18.6 MPa2700 psi
 19.8 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
2870 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Air Oven Aging
Elongation at Break 370 %370 %
 348 %
@Treatment Temp. 200 °C,
Time 252000 sec
348 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Air Oven Aging
100% Modulus 3.10 MPa
@Strain 100 %
450 psi
@Strain 100 %
Compression Set  20 %
@Temperature 175 °C,
Time 252000 sec
20 %
@Temperature 347 °F,
Time 70.0 hour
#214 O-ring; ASTM D395 Method B
 31 %
@Temperature 200 °C,
Time 252000 sec
31 %
@Temperature 392 °F,
Time 70.0 hour
#214 O-ring; ASTM D395 Method B
 
Thermal PropertiesMetricEnglishComments
Minimum Service Temperature, Air -19.0 °C-2.20 °FLow Temperature Retraction, TR10
 -15.5 °C4.10 °FGehman Torsion T10; ASTM 1053-92A
 -10.0 °C14.0 °FLow Temperature Retraction, TR70
 -10.0 °C14.0 °FGehman Torsion T2; ASTM 1053-92A
Brittleness Temperature -25.0 °C-13.0 °FEmbrittlement
 
Processing PropertiesMetricEnglishComments
Cure Time 0.500 min0.00833 hourts2, scorch time
 0.600 min0.0100 hourt'50, time to 50% cure
 0.800 min0.0133 hourt'90, time to 90% cure
 10.0 min
@Temperature 177 °C
0.167 hour
@Temperature 351 °F
Press Cure
 240 min
@Temperature 200 °C
4.00 hour
@Temperature 392 °F
Post cure
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 66 %66 %
 
Descriptive Properties
ColorWhite to light pink
MH18 dNmmaximum torque
ML0.8 dNmminimum torque
Test Formula100 phrDAI-EL® G-684BP
 3 phrPeroxide (50% Activity)
 3 phrZinc Oxide
 30 phrMT Carbon Black (N-990)
 4 phrTAIC (72% Activity)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Daikin DAI-EL® G-755 Fluoroelastomer Copolymer, Bisphenol Curable Grade, 66% Fluorine Content
Daikin DAI-EL® G-755 Fluoroelastomer Copolymer, 66% Fluorine Content
Daikin DAI-EL® G-801 Fluoroelastomer Copolymer, 66% Fluorine Content
Phillips 66 Bentone NLGI Grade 2
Daikin DAI-EL® G-723 Fluoroelastomer Copolymer, Bisphenol Curable Grade, 66% Fluorine Content

PDAIJ9854 / 209925

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.